# US 2023/0407083 A1 · Economical epoxy resin material for epoxy asphalt with low-temperature resistance and high flexibility as well as preparation method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0407083 A1
- Document ID: US20230407083A1
- Status: Published application
- Kind: A1
- Application number: 18/335,100
- Filed: 2023-06-14
- Published: 2023-12-21
- Earliest claimed: 2022-06-16
- Assignees: Southeast University
- Applicants: Southeast University
- Inventors: Sang LUO; Jing HU
- Web page: https://patentgrep.com/patent/US20230407083A1

## CPC

- C04B 26/26: Bituminous materials, e.g. tar, pitch {(C08L95/00 takes precedence)}
- C08L 63/00: Compositions of epoxy resins; Compositions of derivatives of epoxy resins
- C04B 24/281: {Polyepoxides}
- C08G 59/5006: {aliphatic}
- C08G 59/5026: {cycloaliphatic}
- C08J 3/203: {Solid polymers with solid and/or liquid additives}
- C08K 5/098: Metal salts of carboxylic acids
- C08K 5/17: Amines; Quaternary ammonium compounds
- C08K 5/3462: Six-membered rings
- C04B 2111/0075: {for road construction}
- C08J 2363/00: Characterised by the use of epoxy resins; Derivatives of epoxy resins
- Y02A 30/30: in transportation, e.g. on roads, waterways or railways
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE
- C08L: COMPOSITIONS OF MACROMOLECULAR COMPOUNDS (compositions based on polymerisable monomers C08F, C08G; artificial filaments or fibres D01F; textile treating compositions D06)
- C08G: MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
- C08J: WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H (working, e.g. shaping, of plastics B29)
- C08K: Use of inorganic or non-macromolecular organic substances as compounding ingredients (paints, inks, varnishes, dyes, polishes, adhesives C09)
- Y02A: TECHNOLOGIES FOR ADAPTATION TO CLIMATE CHANGE

## Abstract

The present disclosure discloses an economical epoxy resin material for epoxy asphalt with low-temperature resistance and high flexibility as well as a preparation method thereof. The material comprises 60 parts of an epoxy resin main agent, 0.4 parts to 1.6 parts of a modifying gent, 31 parts to 36.5 parts of an active curing agent, 0.5 parts to 1.5 parts of a titanate coupling agent, and 1.6 parts to 6.4 parts of a reversible deformation additive.

## Claims

### Claim 1

An economical epoxy resin material for epoxy asphalt with low-temperature resistance and high flexibility, wherein the material comprises following components by a mass fraction:
a Component A:
60 parts of an epoxy resin main agent;
a Component B:
0.4 parts to 1.6 parts of a modifying agent,
31 parts to 36.5 parts of an active curing agent,
0.5 parts to 1.5 parts of a titanate coupling agent, and
1.6 parts to 6.4 parts of a reversible deformation additive.

### Claim 2 (depends on 1)

The economical epoxy resin material for epoxy asphalt with low-temperature resistance and high flexibility according to claim 1, wherein the epoxy resin main agent is selected from any one or a mixture of diphenol propane glycidyl ether resin and diphenol methane glycidyl ether resin.

### Claim 3 (depends on 1)

The economical epoxy resin material for epoxy asphalt with low-temperature resistance and high flexibility according to claim 1, wherein the modifying agent is selected from any one or a mixture of more than two from 1,8-diamino-p-montane, 1-piperazine ethylamine, 4,4′-diaminodicyclohexylmethane, and 1,3-bis (aminomethyl) cyclohexane.

### Claim 4 (depends on 1)

The economical epoxy resin material for epoxy asphalt with low-temperature resistance and high flexibility according to claim 1, wherein the active curing agent is selected from any one or a mixture of more than two from coco alkyl primary amine, 1-amino-9-octadecene, oleyl amine polyoxyethylene ether and lauroyl glutamic acid.

### Claim 5 (depends on 1)

The economical epoxy resin material for epoxy asphalt with low-temperature resistance and high flexibility according to claim 1, wherein the titanate coupling agent is selected from any one or a mixture of more than two from isopropyl triisostearoyl titanate, isopropyl trilauryl titanate, isopropyl tris (dodecylbenzenesulfonyl) titanate and isopropyl isostearoyl diacryloyl titanate.

### Claim 6 (depends on 1)

The economical epoxy resin material for epoxy asphalt with low-temperature resistance and high flexibility according to claim 1, wherein the reversible deformation additive is selected from any one or a mixture of more than two from acrylonitrile-butadiene rubber, fluorine rubber, liquid acrylate rubber and liquid phenolic resin.

### Claim 7 (depends on 1)

A method for preparing the economical epoxy resin material for epoxy asphalt with low-temperature resistance and high flexibility according to claim 1, comprising following steps:
(1) mixing the active curing agent, the modifying agent, the titanate coupling agent and the reversible deformation additive, preheating the mixture to 60° C., and stirring and mixing the mixture to obtain the component B; and
(2) mixing the component B obtained in Step (1) with the component A and stirring the mixture for 5 minutes at a temperature of 60±5° C. to obtain the epoxy resin material.

### Claim 8 (depends on 7)

The method for preparing the economical epoxy resin material for epoxy asphalt with low-temperature resistance and high flexibility according to claim 7, wherein in Step (1), a stirring temperature for preparing the component B is 80±5° C., and a stirring time is 3 hours.

### Claim 9 (depends on 1)

A use of the epoxy resin material according to claim 1 in preparing an epoxy asphalt for paving highway pavement, concrete bridge pavement and steel bridge pavement.

### Claim 10 (depends on 9)

The use according to claim 9, comprising following steps:
S1: evenly mixing Components A and B in the epoxy resin material;
S2: taking 100 parts of the epoxy resin material obtained by mixing in Step S1 and adding the epoxy resin material into 100 parts of a matrix asphalt, and stirring the mixture at a temperature of 160±10° C. for 5 minutes to obtain the epoxy asphalt;
S3: mixing the epoxy asphalt obtained in Step S2 with an aggregate and a mineral powder, and stirring the mixture for 1 minute to 2 minutes at a temperature of 170±10° C. to obtain an epoxy asphalt mixture; wherein a mass percent of the epoxy asphalt is 4% to 6%, and a mass percent of the aggregate and the mineral powder is 94% to 96%; and
S4: spreading the epoxy asphalt mixture obtained in Step S3 on the pavement or the deck, rolling the epoxy asphalt mixture into shape, and curing the shaped epoxy asphalt mixture at a temperature of 5° C. to 50° C. for 36 hours to 96 hours.