# US 2023/0399051 A1 · Method for producing a welded steel blank and associated welded blank

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0399051 A1
- Document ID: US20230399051A1
- Status: Published application
- Kind: A1
- Application number: 18/450,472
- Filed: 2023-08-16
- Published: 2023-12-14
- Earliest claimed: 2017-11-24
- Assignees: ArcelorMittal
- Applicants: ArcelorMittal
- Inventors: Cristian ALVAREZ; Thierry LIZON; Maria POIRIER
- Web page: https://patentgrep.com/patent/US20230399051A1

## CPC

- B23K 31/02: relating to soldering or welding
- B62D 21/15: having impact absorbing means, e.g. a frame designed to permanently or temporarily change shape or dimension upon impact with another body (bumpers B60R19/02; shock absorbers in general F16F)
- B21D 22/022: {by heating the blank or stamping associated with heat treatment (C21D takes precedence)}
- B23K 26/0006: {taking account of the properties of the material involved (B23K26/32, B23K26/40 take precedence)}
- B23K 26/211: with interposition of special material to facilitate connection of the parts
- B23K 26/24: Seam welding
- B23K 26/26: of rectilinear seams
- B23K 26/322: involving coated metal parts (using absorbing layers on the workpiece B23K26/18)
- B23K 26/60: Preliminary treatment
- B23K 33/00: Specially-profiled edge portions of workpieces for making soldering or welding connections; Filling the seams formed thereby
- B23K 35/24: Selection of soldering or welding materials proper (B23K35/34 takes precedence)
- B23K 35/383: {mainly containing noble gases or nitrogen}
- B62D 27/02: rigid
- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 9/505: {Cooling thereof}
- C22C 19/057: {with the maximum Cr content being less 10%}
- C22C 30/02: containing copper
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/32: with boron
- C22C 38/38: with more than 1.5% by weight of manganese
- B23K 2101/006: {Vehicles}
- B23K 2101/18: Sheet panels
- B23K 2101/185: {Tailored blanks}
- B23K 2101/34: Coated articles {; Surface treated articles}
- B23K 2103/04: Steel {or steel} alloys
- B23K: SOLDERING OR UNSOLDERING; WELDING; CLADDING OR PLATING BY SOLDERING OR WELDING; CUTTING BY APPLYING HEAT LOCALLY, e.g. FLAME CUTTING; WORKING BY LASER BEAM
- B62D: MOTOR VEHICLES; TRAILERS (steering, or guiding on a desired track, of agricultural machines or implements A01B69/00; wheels, castors, axles, increasing wheel adhesion B60B; vehicle tyres, tyre inflation or tyre changing B60C; connections between vehicles of a train or the like B60D; vehicles for use on rail and road, amphibious or convertible vehicles B60F; suspension arrangements B60G; heating, cooling, ventilating or other air treating devices B60H; windows, windscreens, non-fixed roofs, doors or similar devices, protective coverings for vehicles not in use B60J; propulsion plant arrangements, auxiliary drives, transmissions, controls, instrumentation or dashboards B60K; electric equipment or propulsion of electrically-propelled vehicles B60L; power supply for electrically-propelled vehicles B60M; passenger accommodation not otherwise provided for B60N; adaptations for load transportation or to carry special loads or objects B60P; arrangement of signalling or lighting devices, the mounting or supporting thereof or circuits therefor, for vehicles in general B60Q; vehicles, vehicle fittings or vehicle parts not otherwise provided for B60R; servicing, cleaning, repairing, supporting, lifting, or manoeuvring, not otherwise provided for, B60S; brake arrangements, brake control systems or parts thereof B60T; air-cushion vehicles B60V; motor-cycles, accessories therefor B62J, B62K; testing of vehicles G01M)
- B21D: WORKING OR PROCESSING OF SHEET METAL OR METAL TUBES, RODS OR PROFILES WITHOUT ESSENTIALLY REMOVING MATERIAL; PUNCHING METAL (working or processing of wire B21F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

A method for producing a welded blank (1) includes providing two precoated sheets (2), butt welding the precoated sheets (2) using a filler wire. The precoating (5) entirely covers at least one face (4) of each sheet (2) at the time of butt welding. The filler wire (20) has a carbon content between 0.01 wt. % and 0.45 wt. %. The composition of the filler wire (20) and the proportion of filler wire (20) added to the weld pool is chosen such that the weld joint (22) has (a) a quenching factor FTWJ: FTWJ−0.9FTBM≥0, where FTBM is a quenching factor of the least hardenable substrate (3), and FTWJ and FTBM are determined: FT=128+1553×C+55×Mn+267×Si+49×Ni+5×Cr−79×Al−2×Ni2−1532×C2−5×Mn2−127×Si2−40×C×Ni−4×Ni×Mn, and (b) a carbon content CWJ<0.15 wt. % or, if CWJ≥0.15 wt. %, a softening factor FAWJ such that FAWJ>5000, where FA=10291+4384.1×Mo+3676.9Si−522.64×Al−2221.2×Cr−118.11×Ni−1565.1×C−246.67×Mn.

## Claims

### Claim 1

A method for producing a welded steel blank comprising the successive steps of:
providing two precoated sheets, each precoated sheet comprising a steel substrate having a precoating on at least one of its main faces, the precoating comprising an intermetallic alloy layer comprising at least iron and aluminum, the steel substrate being made of a press-hardenable steel, for at least one of the precoated sheets, the steel of the steel substrate comprising, Fe and at least one of C, Mn, Si, Cr, Ti, Al, S, P and B; and
butt welding the precoated sheets using a filler wire so as to form a weld joint at a junction between the precoated sheets, the precoating entirely covering at least one main face of each precoated sheet at a time of butt welding,
the filler wire having a carbon content comprised between 0.01 wt. % and 0.45 wt. %,
a composition of the filler wire and a proportion of filler wire added to a weld pool is chosen in such a manner that the thus obtained weld joint is characterized by:
(a) a quenching factor FTWJ of the weld joint such that FTWJ−0.9FTBM≥0, where:
FTBM is the quenching factor of a least hardenable steel substrate among the steel substrates of the two precoated sheets, and
the quenching factors FTWJ and FTBM are determined using the following formula: FT=128+1553×C+55×Mn+267×Si+49×Ni+5×Cr−79×Al−2×Ni2−1532×C2−5×Mn2−127×Si2−40×C×Ni−4×Ni×Mn, where Al, Cr, Ni, C, Mn and Si are, respectively, a mean aluminum, chromium, nickel, carbon, manganese and silicon content, expressed in weight percent, of an area whose quenching factor is to be determined, this area being the weld joint in the case of FTWJ and the least hardenable steel substrate in the case of FTBM, and
(b) a carbon content CWJ of the weld joint strictly smaller than 0.15 wt. % or, if the carbon content CWJ of the weld joint is greater than or equal to 0.15 wt. %, a softening factor FAWJ of the weld joint such that FAWJ>5000, where the softening factor FAWJ of the weld joint is calculated as a function of a mean aluminum, chromium, nickel, molybdenum, carbon, manganese and silicon content of the weld joint, expressed in weight percent, using the following formula:
FA=10291+4384.1×Mo+3676.9Si−522.64×Al−2221.2×Cr−118.11×Ni−1565.1×C−246.67×Mn.

### Claim 2 (depends on 1)

The method as recited in claim 1, wherein each of the steel substrates has a thickness comprised between 0.8 mm and 5 mm, and for at least one of the precoated sheets, the steel of the steel substrate comprises, by weight:
0.10%≤C≤0.5%
0.5%≤Mn≤3%
0.1%≤Si≤1%
0.01%≤Cr≤1%
Ti≤0.2%
Al≤0.1%
S≤0.05%
P≤0.1%
B≤0.010%
a rest being iron and impurities resulting from manufacturing.

### Claim 3 (depends on 1)

The method as recited in claim 1, wherein, for each of the precoated sheets, the steel of the steel substrate comprises, by weight:
0.10%≤C≤0.5%
0.5%≤Mn≤3%
0.1%≤Si≤1%
0.01%≤Cr≤1%
Ti≤0.2%
Al≤0.1%
S≤0.05%
P≤0.1%
B≤0.010%
a rest being iron and impurities resulting from manufacturing.

### Claim 4 (depends on 1)

The method as recited in claim 1, wherein the precoating further comprises a metallic alloy layer extending atop the intermetallic alloy layer, the metallic alloy layer being a layer of aluminum, a layer of aluminum alloy or a layer of aluminum-based alloy.

### Claim 5 (depends on 1)

The method as recited in claim 1, wherein the carbon content CWJ, in weight percent, of the weld joint is such that 1.25λCBM(most hardenable)−CWJ≥0, where CBM is the carbon content, in weight percent, of a most hardenable steel substrate among the steel substrates of the two precoated sheets.

### Claim 6 (depends on 1)

The method as recited in claim 1, wherein a nickel content NiWJ of the weld joint is comprised between 2.0 wt. % and 11.0 wt. %.

### Claim 7 (depends on 1)

The method as recited in claim 1, wherein the carbon content CWJ, in weight percent, of the weld joint is such that 1.25λCBM(most hardenable)−CWJ≥0, where CBM is the carbon content, in weight percent, of a most hardenable steel substrate among the steel substrates of the two precoated sheets, a nickel content NiWJ of the weld joint being comprised between 2.0 wt. % and 11.0 wt. %.

### Claim 8 (depends on 1)

The method as recited in claim 1, wherein the precoated sheets provided in the providing step each have the precoating on both of their main faces.

### Claim 9 (depends on 8)

The method as recited in claim 8, wherein, at the time of butt welding, the precoating remains integrally on both main faces of at least one of the precoated sheets.

### Claim 10 (depends on 1)

The method as recited in claim 1, further comprising, prior to butt welding, preparing a weld edge of at least one of the precoated sheets for incorporating at least partially into the weld joint, using at least one of the following processing steps:
brushing, machining, chamfering, bevelling and/or removing at least a portion of the precoating,
the preparation being performed in such a manner that the precoating remains integrally on at least one main face of each of the two precoated sheets.

### Claim 11 (depends on 1)

The method as recited in claim 1, wherein the welding step is performed exclusively using a laser beam.

### Claim 12 (depends on 1)

The method as recited in claim 1, wherein, for at least one of the precoated sheets, the steel of the steel substrate comprises, by weight:
0.15%≤C≤0.25%
0.8%≤Mn≤1.8%
0.1%≤Si≤0.35%
0.01%≤Cr≤0.5%
Ti≤0.1%
Al≤0.1%
S≤0.05%
P≤30.1%
B≤0.005%
a rest being iron and impurities resulting from manufacturing.

### Claim 13 (depends on 1)

The method as recited in claim 1, wherein, for at least one of the precoated sheets, the steel of the steel substrate comprises, by weight:
0.24%≤C≤0.38%
0.40%≤Mn≤3%
0.10%≤Si≤0.70%
0.015%≤AI≤0.070%
0%≤Cr≤2%
0.25%≤Ni≤2%
0.015%≤Ti≤0.10%
0%≤Nb≤0.060%
0.0005%≤B≤0.0040%
0.003%≤N≤0.010%
0.0001%≤S≤0.005%
0.0001%≤P≤0.025%
wherein the titanium and nitrogen contents satisfy the following relationship:
Ti/N>3.42.
and the carbon, manganese, chromium and silicon contents satisfy the following relationship:
2.6
C
+
Mn
5.3
+
Cr
13
+
Si
15
≥
1.1
%
,
the steel optionally comprising one or more of the following elements:
0.05%≤Mo≤0.65%
0.001%≤W≤0.30%%
0.0005%≤Ca≤0.005%
a rest being iron and impurities resulting from manufacturing.

### Claim 14 (depends on 1)

The method as recited in claim 1, wherein the welding is performed using a protection gas.

### Claim 15 (depends on 14)

The method as recited in claim 14, wherein the protection gas is helium and/or argon.

### Claim 16 (depends on 1)

A method for producing a welded and thereafter hot press-formed and cooled steel part comprising the successive steps of:
carrying out the method as recited in claim 1 in order to obtain the welded steel blank;
heating the welded steel blank so as to obtain a fully austenitic structure in the steel substrates of the precoated sheets;
hot press-forming the welded steel blank in a press tool to obtain a steel part; and
cooling the steel part in the press tool.

### Claim 17 (depends on 16)

The method according to claim 16, wherein, during the cooling step, a cooling rate is greater than or equal to a bainitic or martensitic cooling rate of a most hardenable among the steel substrates of the precoated sheets.

### Claim 18

A welded steel blank comprising:
two precoated sheets, each precoated sheet comprising a steel substrate having a precoating on at least one of its main faces, the precoating comprising an intermetallic alloy layer comprising at least iron and aluminum, the steel substrate being made of a press-hardenable steel,
for at least one of the precoated sheets, the steel of the steel substrate comprising, Fe and at least one of C, Mn, Si, Cr, Ti, Al, S, P and B, and
the precoated sheets being joined by a weld joint, the weld joint being characterized by:
(a) a quenching factor FTWJ of the weld joint such that FTWJ−0.9FTBM≥0, where:
FTBM is the quenching factor of a least hardenable steel substrate among the steel substrates of the two precoated sheets, and
the quenching factors FTWJ and FTBM are determined using the following formula: FT=128+1553×C+55×Mn+267×Si+49×Ni+5×Cr−79×Al−2×Ni2−1532×C2−5×Mn2−127×Si2−40×C×Ni−4×Ni×Mn, where Al, Cr, Ni, C, Mn and Si are, respectively, a mean aluminum, chromium, nickel, carbon, manganese and silicon content, expressed in weight percent, of an area whose quenching factor is to be determined, this area being the weld joint in the case of FTWJ and the least hardenable steel substrate in the case of FTBM, and
(b) a carbon content CWJ of the weld joint strictly smaller than 0.15 wt. % or, if the carbon content CWJ of the weld joint is greater than or equal to 0.15 wt. %, a softening factor FAWJ of the weld joint such that FAWJ>5000, where the softening factor FAWJ of the weld joint is calculated as a function of a mean aluminum, chromium, nickel, molybdenum, carbon, manganese and silicon content of the weld joint, expressed in weight percent, using the following formula:
FA=10291+4384.1×Mo+3676.9Si−522.64×Al−2221.2×Cr−118.11×Ni−1565.1×C−246.67×Mn,
and the weld joint is such that, after hot press-forming and cooling, a maximum hardness variation ΔHV(WJ) across the weld joint is smaller than or equal to 20% of a mean hardness HVmean (WJ) of the weld joint.

### Claim 19 (depends on 18)

The welded steel blank as recited in claim 18, wherein each of the steel substrates has a thickness comprised between 0.8 mm and 5 mm, and for at least one of the precoated sheets, the steel of the steel substrate comprises, by weight:
0.10%≤C≤0.5%
0.5%≤Mn≤3%
0.1%≤Si≤1%
0.01%≤Cr≤1%
Ti≤0.2%
Al≤0.1%
S≤0.05%
P≤0.1%
B≤0.010%
a rest being iron and impurities resulting from manufacturing.

### Claim 20 (depends on 18)

The welded steel blank as recited in claim 18, wherein, for each of the precoated sheets, the steel of the steel substrate comprises, by weight:
0.10%≤C≤0.5%
0.5%≤Mn≤3%
0.1%≤Si≤1%
0.01%≤Cr≤1%
Ti≤0.2%
Al≤0.1%
S≤0.05%
P≤0.1%
B≤0.010%
a rest being iron and impurities resulting from manufacturing.

### Claim 21 (depends on 18)

The welded steel blank as recited in claim 18, wherein the precoating further comprises a metallic alloy layer extending atop the intermetallic alloy layer, the metallic alloy layer being a layer of aluminum, a layer of aluminum alloy or a layer of aluminum-based alloy.

### Claim 22 (depends on 18)

The welded steel blank as recited in claim 18, wherein the carbon content CWJ, in weight percent, of the weld joint is such that 1.25×CBM(most hardenable)−CWJ≥0, where CBM is the carbon content, in weight percent, of a most hardenable steel substrate among the steel substrates of the two precoated sheets.

### Claim 23 (depends on 18)

The welded steel blank as recited in claim 18, wherein a nickel content NiWJ of the weld joint is comprised between 2.0 wt. % and 11.0 wt. %.

### Claim 24 (depends on 18)

The welded steel blank as recited in claim 18, wherein the carbon content CWJ, in weight percent, of the weld joint is such that 1.25×CBM(most hardenable)−CWJ≥0, where CBM is the carbon content, in weight percent, of a most hardenable steel substrate among the steel substrates of the two precoated sheets, a nickel content NiWJ of the weld joint being comprised between 2.0 wt. % and 11.0 wt. %.

### Claim 25 (depends on 18)

The welded steel blank as recited in claim 18, wherein the weld joint is obtained exclusively through laser welding.

### Claim 26 (depends on 18)

The welded steel blank as recited in claim 18, wherein for at least one of the precoated sheets, the steel of the steel substrate comprises, by weight:
0.15%≤C≤0.25%
0.8%≤Mn≤1.8%
0.1%≤Si≤0.35%
0.01%≤Cr≤0.5%
Ti≤0.1%
Al≤0.1%
S≤0.05%
P≤0.1%
B≤0.005%
a rest being iron and impurities resulting from manufacturing.

### Claim 27 (depends on 18)

The welded steel blank as recited in claim 18, wherein for one of the precoated sheets, the steel of the steel substrate comprises, by weight:
0.24%≤C≤0.38%
0.40%≤Mn≤3%
0.10%≤Si≤0.70%
0.015%≤AI≤0.070%
0%≤Cr≤2%
0.25%≤Ni≤2%
0.015%≤Ti≤0.10%
0%≤Nb≤0.060%
0.0005%≤B≤0.0040%
0.003%≤N≤0.010%
0.0001%≤S≤0.005%
0.0001%≤P≤0.025%
wherein the titanium and nitrogen contents satisfy the following relationship
Ti/N>3.42.
and the carbon, manganese, chromium and silicon contents satisfy the following relationship:
2.6
C
+
Mn
5.3
+
Cr
13
+
Si
15
≥
1.1
%
,
the steel optionally comprising one or more of the following elements:
0.05%≤Mo≤0.65%
0.001%≤W≤0.30%%
0.0005%≤Ca≤0.005%
a rest being iron and impurities resulting from manufacturing; and
wherein for the other of the precoated sheets, the steel of the steel substrate comprises, by weight:
0.10%≤C≤0.5%
0.5%≤Mn≤3%
0.1%≤Si≤1%
0.01%≤Cr≤1%
Ti≤0.2%
Al≤0.1%
S≤0.05%
P≤0.1%
B≤0.010%
a rest being iron and impurities resulting from manufacturing.

### Claim 28

A welded, hot press-formed and cooled steel part comprising:
a first coated steel part portion; and
a second coated steel part portion,
each coated steel part portion comprising a steel substrate having, on at least one of its main faces, a coating comprising at least iron and aluminum, the steel substrate being made of a press-hardenable steel,
the steel of the steel substrate of at least one among the first and the second coated steel part portions comprising Fe and at least one of C, Mn, Si, Cr, Ti, Al, S, P and B, and
and the first and second coated steel part portions being joined by a weld joint, the weld joint being characterized by:
(a) a quenching factor FTWJ of the weld joint such that FTWJ−0.9FTBM≥0, where:
FTBM is the quenching factor of a least hardenable steel substrate among the steel substrates of the two coated steel part portions, and
the quenching factors FTWJ and FTBM are determined using the following formula: FT=128+1553×C+55×Mn+267×Si+49×Ni+5×Cr−79×Al−2×Ni2−1532×C2−5×Mn2−127×Si2−40×C×Ni−4×Ni×Mn, where Al, Cr, Ni, C, Mn and Si are, respectively, a mean aluminum, chromium, nickel, carbon, manganese and silicon content, expressed in weight percent, of an area whose quenching factor is to be determined, this area being the weld joint in the case of FTWJ and the least hardenable steel substrate in the case of FTBM, and
(b) a carbon content CWJ of the weld joint strictly smaller than 0.15 wt. % or, if the carbon content CWJ of the weld joint is greater than or equal to 0.15 wt. %, a softening factor FAWJ of the weld joint such that FAWJ>5000, where the softening factor FAWJ of the wed joint is calculated as a function of a mean aluminum, chromium, nickel, molybdenum, carbon, manganese and silicon content of the weld joint, expressed in weight percent, using the following formula:
FA=10291+4384.1×Mo+3676.9Si−522.64×Al−2221.2×Cr−118.11×Ni−1565.1×C−246.67×Mn
and a maximum hardness variation ΔHV(WJ) across the weld joint is smaller than or equal to 20% of a mean hardness HVmean (WJ) of the weld joint.

### Claim 29 (depends on 28)

The welded, hot press-formed and cooled steel part as recited in claim 28, wherein each of the steel substrates has a thickness comprised between 0.8 mm and 5 mm, and the steel of the steel substrate of at least one among the first and the second coated steel part portions comprises, by weight:
0.10%≤C≤0.5%
0.5%≤Mn≤3%
0.1%≤Si≤1%
0.01%≤Cr≤1%
Ti≤0.2%
Al≤0.1%
S≤0.05%
P≤0.1%
B≤0.010%
a rest being iron and impurities resulting from manufacturing.

### Claim 30 (depends on 28)

The welded, hot press-formed and cooled steel part as recited in claim 28, wherein, the steel of the steel substrate of at least one among the first and the second coated steel part portions comprises, by weight:
0.10%≤C≤0.5%
0.5%≤Mn≤3%
0.1%≤Si≤1%
0.01%≤Cr≤1%
Ti≤0.2%
Al≤0.1%
S≤0.05%
P≤0.1%
B≤0.010%
a rest being iron and impurities resulting from manufacturing.

### Claim 31 (depends on 28)

The welded, hot press-formed and cooled steel part as recited in claim 28, wherein a hardness drop in a Heat Affected Zone relative to a base metal of the first and second coated steel part portions adjacent thereto is smaller than or equal to 8%.

### Claim 32 (depends on 28)

The welded, hot press-formed and cooled steel part as recited in claim 28, wherein the mean hardness HVmean (WJ) in the weld joint is smaller than or equal to 600 HV.

### Claim 33 (depends on 28)

The welded, hot press-formed and cooled steel part as recited in claim 28, wherein the carbon content CWJ, in weight percent, in the weld joint is such that 1.25×CBM−CWJ≥0, where CBM is the carbon content, in weight percent, of a most hardenable steel substrate among the steel substrates of the first and second coated steel part portions.

### Claim 34 (depends on 28)

The welded, hot press-formed and cooled steel part as recited in claim 28, wherein the nickel content NiWJ in the weld joint is comprised between 2.0 wt. % and 11.0 wt. %.

### Claim 35 (depends on 28)

The welded, hot press-formed and cooled steel part as recited in claim 28, wherein the carbon content CWJ, in weight percent, in the weld joint is such that 1.25×CBM−CWJ≥0, where CBM is the carbon content, in weight percent, of a most hardenable steel substrate among the steel substrates of the first and second coated steel part portions, the nickel content NiWJ in the weld joint being comprised between 2.0 wt. % and 11.0 wt. %.

### Claim 36 (depends on 28)

The welded, hot press-formed and cooled steel part as recited in claim 28, wherein, the steel of the steel substrate of at least one among the first and the second coated steel part portions comprises, by weight:
0.15%≤C≤0.25%
0.8%≤Mn≤1.8%
0.1%≤Si≤0.35%
0.01%≤Cr≤0.5%
Ti≤0.1%
Al≤0.1%
S≤0.05%
P≤0.1%
B≤0.005%
a rest being iron and impurities resulting from manufacturing.

### Claim 37 (depends on 28)

The welded, hot press-formed and cooled steel part as recited in claim 28, wherein the steel of the steel substrate of at least one among the first and the second coated steel part portions comprises, by weight:
0.24%≤C≤0.38%
0.40%≤Mn≤3%
0.10%≤Si≤0.70%
0.015%≤AI≤0.070%
0%≤Cr≤2%
0.25%≤Ni≤2%
0.015%≤Ti≤0.10%
0%≤Nb≤0.060%
0.0005%≤B≤0.0040%
0.003%≤N≤0.010%
0.0001%≤S≤0.005%
0.0001%≤P≤0.025%
wherein the titanium and nitrogen contents satisfy the following relationship
Ti/N>3.42.
and the carbon, manganese, chromium and silicon contents satisfy the following relationship
2.6
C
+
Mn
5.3
+
Cr
13
+
Si
15
≥
1.1
%
,
the steel optionally comprising one or more of the following elements:
0.05%≤Mo≤0.65%
0.001%≤W≤0.30%%
0.0005%≤Ca≤0.005%
a rest being iron and impurities resulting from manufacturing.

### Claim 38 (depends on 28)

A method of producing a motor vehicle part comprising:
producing an anti-intrusion part or an energy-absorption part for a motor vehicle using the welded, hot press-formed and cooled steel part according to claim 28.