# US 2023/0357892 A1 · Method for making tungsten-refactory metal alloy powder and tungsten-refractory metal alloy powders made by the method

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0357892 A1
- Document ID: US20230357892A1
- Status: Published application
- Kind: A1
- Application number: 17/786,428
- Filed: 2020-12-04
- Published: 2023-11-09
- Earliest claimed: 2019-12-19
- Assignees: Rhenium Alloys, Inc.
- Applicants: Rhenium Alloys, Inc.
- Inventors: Todd LEONHARDT
- Web page: https://patentgrep.com/patent/US20230357892A1

## CPC

- C22C 1/1084: {by mechanical alloying (blending, milling)}
- B22F 1/065: Spherical particles
- B22F 1/09: {Mixtures of metallic powders}
- B22F 1/12: Metallic powder containing non-metallic particles (containing lubricating or binding agents or organic material B22F1/10)
- B22F 1/142: Thermal or thermo-mechanical treatment
- B22F 3/15: Hot isostatic pressing
- B22F 9/04: starting from solid material, e.g. by crushing, grinding or milling ({C22C1/1084 takes precedence}; crushing, grinding or milling, in general, see the relevant subclasses, e.g. B02C)
- C22C 1/059: Making alloys comprising less than 5% by weight of dispersed reinforcing phases
- C22C 27/04: Alloys based on tungsten or molybdenum
- C22C 32/0047: {with carbides, nitrides, borides or silicides as the main non-metallic constituents}
- C22C 32/0052: {only carbides}
- B22F 1/05: Metallic powder characterised by the size or surface area of the particles
- B22F 2009/041: {by mechanical alloying, e.g. blending, milling}
- B22F 2009/043: {by ball milling}
- B22F 2301/20: Refractory metals
- B22F 2302/10: Carbide
- B22F 2303/01: Main component
- B22F 2303/05: Compulsory alloy component
- B22F 2304/10: Micron size particles, i.e. above 1 micrometer up to 500 micrometer
- B22F 2998/10: Processes characterised by the sequence of their steps
- B22F 2999/00: Aspects linked to processes or compositions used in powder metallurgy
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- B22F: WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER (making alloys by powder metallurgy C22C); APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER

## Abstract

A method for forming tungsten-refractory metal alloy powders, and tungsten-refractory metal alloy powders formed by the method. The method includes mixing a majority portion by weight of a base tungsten powder with a minority portion by weight of a base refractory metal powder to form a mixture, which is then milled for a period of time sufficient to at least partially mechanically alloy the base tungsten powder and base refractory metal powder together to form at-least-partially-mechanically-alloyed particles, which are then heat treated to a temperature sufficient to promote diffusion between tungsten and the refractory metal and obtain agglomerations of particles having only a tungsten phase, which are then milled to break up the agglomerations of particles and obtain the tungsten-refractory metal alloy powder.

## Claims

### Claim at position 1

1-29. (canceled)

### Claim 30

A method for forming a tungsten-refractory metal alloy powder, the method comprising the steps of:
(a) mixing a majority portion by weight of a base tungsten powder with a minority portion by weight of a base refractory metal powder to form a mixture, said base refractory metal powder being formed of a refractory metal other than tungsten;
(b) milling the mixture from step (a) for a period of time sufficient to at least partially mechanically alloy the base tungsten powder and base refractory metal powder together to form at-least-partially-mechanically-alloyed particles;
(c) heat treating the at-least-partially-mechanically-alloyed particles from step (b) to a temperature sufficient to promote diffusion between tungsten and the refractory metal other than tungsten and obtain agglomerations of particles having only a tungsten phase; and
(d) milling the agglomerations of particles having only a tungsten phase from step (c) to break up the agglomerations of particles and obtain the tungsten-refractory metal alloy powder.

### Claim 31 (depends on 30)

The method according to claim 30, wherein the base refractory metal powder in step (a) is rhenium powder, and wherein the rhenium powder in step (a) comprises from about 20% to about 25.75% of the mixture by weight.

### Claim 32 (depends on 31)

The method according to claim 31, further comprising adding hafnium carbide powder to the mixture in step (a), and wherein the amount of the hafnium carbide powder added to the mixture in step (a) is such that the hafnium carbide powder comprises up to 4% of the mixture by weight.

### Claim 33 (depends on 30)

The method according to claim 30, wherein the base refractory metal powder in step (a) is molybdenum powder, and wherein the molybdenum powder in step (a) comprises from about 20% to about 40% of the mixture by weight.

### Claim 34 (depends on 33)

The method according to claim 33, further comprising adding zirconium oxide powder to the mixture in step (a), and wherein the amount of zirconium oxide powder added to the mixture in step (a) is such that the zirconium oxide powder comprises up to 2% of the mixture by weight.

### Claim 35 (depends on 30)

The method according to claim 30, wherein the milling in step (b) is performed using a planetary ball mill that uses stainless steel jars and stainless steel and/or tungsten carbide balls as milling media.

### Claim 36 (depends on 30)

The method according to claim 30, wherein the period of time in step (b) is less than 24 hours.

### Claim 37 (depends on 30)

The method according to claim 30, wherein the period of time in step (b) is less than 8 hours.

### Claim 38 (depends on 30)

The method according to claim 30, wherein the at-least-partially-mechanically-alloyed particles have an average particle size (D50) of less than about 20 microns after step (b).

### Claim 39 (depends on 30)

The method according to claim 30, wherein the at-least-partially-mechanically-alloyed particles from step (b) are heated at a temperature of from about 1,000° C. to about 1,700° C. for about 1 hour to about 12 hours in step (c).

### Claim 40 (depends on 30)

The method according to claim 30, wherein the milling in step (d) is performed using a planetary ball mill that uses stainless steel jars and stainless steel and/or tungsten carbide balls as milling media.

### Claim 41 (depends on 30)

The method according to claim 30, wherein the milling in step (d) is performed for a period of time less than 24 hours.

### Claim 42 (depends on 30)

The method according to claim 30, wherein the milling in step (d) is performed for a period of time less than 8 hours.

### Claim 43 (depends on 30)

The method according to claim 30, wherein the tungsten-refractory metal alloy powder has an average particle size (D50) of less than about 20 microns after step (d).

### Claim 44 (depends on 30)

The method according to claim 30, wherein:
(i) the base refractory metal powder in step (a) is rhenium powder;
(ii) the rhenium powder in step (a) comprises from about 25±1% of the mixture by weight;
(iii) the period of time in step (b) is less than 8 hours;
(iv) the at-least-partially-mechanically-alloyed particles have an average particle size (D50) of less than about 20 microns after step (b);
(v) the at-least-partially-mechanically-alloyed particles from step (b) are heated at a temperature of from about 1,600° C. to about 1,700° C. for about 1 hour to about 12 hours in step (c);
(vi) the milling in step (d) is performed for a period of time less than 8 hours; and
(vii) the tungsten-refractory metal alloy powder has an average particle size (D50) of less than about 16 microns after step (d).

### Claim 45 (depends on 44)

The method according to claim 44, further comprising adding hafnium carbide powder to the mixture in step (a) such that the hafnium carbide powder comprises up to 2% of the mixture by weight.

### Claim 46 (depends on 30)

The method according to claim 30, wherein:
(i) the base refractory metal powder in step (a) is molybdenum powder;
(ii) the molybdenum powder in step (a) comprises from about 30±1% of the mixture by weight;
(iii) the period of time in step (b) is less than 8 hours;
(iv) the at-least-partially-mechanically-alloyed particles from step (b) have an average particle size (D50) of less than about 20 microns after step (b);
(v) the at-least-partially-mechanically-alloyed particles from step (b) are heated at a temperature of from about 1,600° C. to about 1,700° C. for about 1 hour to about 12 hours in step (c);
(vi) the milling in step (d) is performed for a period of time less than 8 hours; and
(vii) the tungsten-refractory metal alloy powder has an average particle size (D50) of less than about 16 microns after step (d).

### Claim 47 (depends on 46)

The method according to claim 46, further comprising adding zirconium oxide powder to the mixture in step (a) such that the zirconium oxide powder comprises up to 2% of the mixture by weigh.

### Claim 48 (depends on 30)

The method according to claim 30, further comprising forming spherical particles comprising the tungsten-refractory metal alloy powder obtained after step (d) by spray freeze drying.

### Claim 49 (depends on 30)

A tungsten-refractory metal alloy powder formed according to the method of claim 30.