# US 2023/0332264 A1 · High-grade non-oriented silicon steel and production method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0332264 A1
- Document ID: US20230332264A1
- Status: Published application
- Kind: A1
- Application number: 18/247,814
- Filed: 2021-07-19
- Published: 2023-10-19
- Earliest claimed: 2020-12-16
- Assignees: Institute of Research of Iron and Steel, Jiangsu Province/Sha-Steel, Co. Ltd (Cn); Zhangjiagang Yangtze River Cold Rolled Plate Co. Ltd; Jiangsu Shagang Group Co., Ltd.
- Applicants: Institute of Research of Iron and Steel, Jiangsu Province/Sha-Steel, Co. Ltd (Cn); Zhangjiagang Yangtze River Cold Rolled Plate Co. Ltd; Jiangsu Shagang Group Co., Ltd.
- Inventors: Chongxiang YUE; Shengjie WU; Jiadong LU; Hui LI
- Web page: https://patentgrep.com/patent/US20230332264A1

## CPC

- C21D 9/46: for sheet metals
- C21D 9/52: for wires; for strips {; for rods of unlimited length}
- B22D 11/001: {of specific alloys}
- C21C 7/0006: {Adding metallic additives}
- C21C 7/068: Decarburising
- C21C 7/10: Handling in a vacuum
- C21D 1/60: Aqueous agents
- C21D 1/76: Adjusting the composition of the atmosphere
- C21D 6/004: {containing Cr and Ni}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0263: {following hot rolling}
- C21D 8/0278: involving a particular surface treatment (C21D8/0294 takes precedence)
- C21D 8/1205: involving particular fabrication steps or treatments of ingots or slabs
- C21D 8/1222: {Hot rolling}
- C21D 8/1261: {following hot rolling}
- C21D 8/1272: {Final recrystallisation annealing}
- C21D 8/1277: involving a particular surface treatment (C21D8/1294 takes precedence)
- C22C 33/04: by melting
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/004: {Very low carbon steels, i.e. having a carbon content of less than 0,01%}
- C22C 38/008: {containing tin}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/34: with more than 1.5% by weight of silicon
- C22C 38/42: with copper
- C22C 38/44: with molybdenum or tungsten
- C22C 38/46: with vanadium
- C22C 38/48: with niobium or tantalum
- C22C 38/50: with titanium or zirconium
- C23G 1/08: Iron or steel
- C23G 3/029: {for removing the pickling fluid from the objects}
- C22C 2202/02: Magnetic
- Y02P 10/20: Recycling
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- B22D: CASTING OF METALS; CASTING OF OTHER SUBSTANCES BY THE SAME PROCESSES OR DEVICES (shaping of plastics or substances in a plastic state B29C; metallurgical processing, selection of substances to be added to metal C21, C22)
- C21C: PROCESSING OF PIG-IRON, e.g. REFINING, MANUFACTURE OF WROUGHT-IRON OR STEEL; TREATMENT IN MOLTEN STATE OF FERROUS ALLOYS
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23G: CLEANING OR DE-GREASING OF METALLIC MATERIAL BY CHEMICAL METHODS OTHER THAN ELECTROLYSIS
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

A high-grade non-oriented silicon steel and a production method are provided. The non-oriented silicon steel includes the following chemical components in percent by mass: 0.002-0.004% of C, not greater than 0.003% of S, 1.4-1.7% of Si, 0.7-0.95% of Mn, not greater than 0.03% of P, 0.015-0.035% of Sn; and 11×([Si]-1.4%)=14×([Mn]-0.7%). In the production method, the heating temperature of a continuous casting billet is 1,120-1,150° C.; the finishing temperature in finish rolling is 890±15° C.; the rolling reduction of the last pass of finish rolling is not less than 30%, the total rolling reduction of the last two passes of finish rolling is not less than 50%, and the coiling temperature is 650±20° C.; normalizing treatment is avoided before acid continuous rolling.

## Claims

### Claim 1

A production method of high-grade non-oriented silicon steel, comprising the following steps:
1) smelting steel by molten iron desulfurization, converter smelting and RH refining in sequence, the finally obtained molten steel comprising the following chemical components in percent by mass: 0.002-0.004% of C, not greater than 0.003% of S, 1.4-1.7% of Si, 0.7-0.95% of Mn, not greater than 0.03% of P, 0.015-0.035% of Sn, not greater than 0.004% of Nb, not greater than 0.004% of V, not greater than 0.005% of Ti, not greater than 0.004% of Mo, not greater than 0.03% of Cr, not greater than 0.03% of Ni, not greater than 0.03% of Cu, not greater than 0.003% of N, and the balance Fe and inevitable impurities, and 11×([Si]-1.4%)=14×([Mn]-0.7%);
2) continuously casting the molten steel obtained in step 1 into a continuous casting billet with the thickness of more than 200 mm;
3) heating the continuous casting billet obtained in step 2 to reach 1,120-1,150° C., and maintaining the temperature for more than 200 min; then carrying out multi-pass rough rolling to obtain an intermediate billet with the thickness of 40-45 mm; and then carrying out multi-pass finish rolling, cooling and coiling to obtain a hot-rolled coil with the thickness of 2.50±0.1 mm, the finishing temperature in finish rolling being 890±15° C., the rolling reduction of the last pass of finish rolling being not less than 30%, the total rolling reduction of the last two passes of finish rolling being not less than 50%, and the coiling temperature being 650±20° C.;
4) carrying out uncoiling, acid pickling, rinsing, drying, cold rolling and coiling on the hot-rolled coil obtained in step 3, rather than carrying out normalizing treatment, thereby obtaining a cold hard coil with the thickness of 0.500±0.005 mm or 0.350±0.004 mm; and
5) carrying out finished product annealing on the cold hard coil obtained in step 4 in a mixed atmosphere of H2+N2 through a continuous annealing furnace, the finished product annealing temperature being 920-980° C., and the annealing time being 60±5 s; and carrying out cooling, coating and finishing on the annealed steel strip to obtain a finished product of non-oriented silicon steel.

### Claim 2 (depends on 1)

The production method of the high-grade non-oriented silicon steel according to claim 1, wherein in a case that the thickness of the finished product of the non-oriented silicon steel is 0.500±0.005 mm, the iron loss is shown as P1.5/50≤3.8 W/kg, and the magnetic induction intensity is shown as B5000≥1.71;
or, in a case that the thickness of the finished product of the non-oriented silicon steel is 0.350±0.004 mm, the iron loss is shown as P1.5/50≤3.3 W/kg, and the magnetic induction intensity is shown as B5000≥1.70.

### Claim 3 (depends on 1)

The production method of the high-grade non-oriented silicon steel according to claim 1, wherein in step 3, the continuous casting billet obtained in step 2 is heated to reach 1,130-1,150° C., and the temperature is maintained for more than 200 min.

### Claim 4 (depends on 1)

The production method of the high-grade non-oriented silicon steel according to claim 1, wherein in step 3, in the cooling process, two-stage cooling is carried out on the steel plate obtained by finishing in finish rolling, the previous-stage cooling is natural slow cooling without water cooling and lasts for 3-8 s, and the later-stage cooling is water-cooling rapid cooling.

### Claim 5 (depends on 1)

The production method of the high-grade non-oriented silicon steel according to claim 1, wherein in the molten iron desulphurization process, the temperature of desulphurized molten iron is controlled to be not less than 1,320° C., the content of S is not greater than 0.0015% by mass, and the slagging-off rate is not less than 98%;
in the converter smelting process, the desulphurized molten iron is mixed with scrap steel to be smelted in a converter, and the scrap steel accounts for 20-25% of the total mass of the molten steel; in the tapping process, a sufficient quantity of tin ingots are added into the molten steel according to the ratio of 0.015-0.035% of Sn in the finished product; and after tapping is finished, a slag top deoxidizing agent is added into the molten steel;
in the RH refining process, the molten steel is subjected to decarburization treatment in a pre-vacuumized RH refining furnace; then ultra-low titanium ferrosilicon and metal manganese are added into the molten steel according to an alloying solution that the finished product contains 1.4-1.7% of Si, and 0.7-0.95% of Mn, and 11×([Si]-1.4%)=14×([Mn]-0.7%); tapping is carried out more than 7 min after net circulation; and a desulfurizing agent is added into the molten steel for deep desulfurization treatment during net circulation.

### Claim 6 (depends on 1)

The production method of the high-grade non-oriented silicon steel according to claim 1, wherein in the acid pickling process, the hot-rolled coil obtained in step 3 is uncoiled and then subjected to three-stage acid pickling through HCl; wherein the concentration of first-stage acid liquor is 50-80 g/L, and the concentration of Fe2+ in the acid liquor is not greater than 130 g/L; the concentration of second-stage acid liquor is 90-120 g/L, and the concentration of Fe2+ in the acid liquor is not greater than 90 g/L; the concentration of third-stage acid liquor is 140-160 g/L, and the concentration of Fe2+ in the acid liquor is not greater than 50 g/L;
during each-stage acid pickling, the temperature of the acid liquor is 75-85° C., the acid liquor contains a silicon steel acid pickling accelerant, and the silicon steel acid pickling accelerant accounts for 0.05-0.10% of the acid liquor by weight; and
the temperature of rinsing water is 45-55° C., and the acid pickling and rinsing speed is controlled to be 100-180 mpm.

### Claim 7 (depends on 1)

The production method of the high-grade non-oriented silicon steel according to claim 1, wherein in step 5, the steel strip obtained after finished product annealing is subjected to three-stage cooling; the first-stage cooling is high-temperature-stage slow cooling, and the steel strip is cooled from annealing temperature to 850° C. at a cooling speed of not greater than 5° C./s; the second-stage cooling is circulating gas jet controlled cooling, and the steel strip is continuously cooled from 850° C. to 350° C. or below at a cooling speed of not greater than 15° C./s; and the third-stage cooling is circulating water jet cooling, and the steel strip is continuously cooled from 350° C. to 100° C. or below.

### Claim 8

A production method of high-grade non-oriented silicon steel, comprising the following steps:
1) smelting steel by molten iron desulfurization, converter smelting and RH refining in sequence, the finally obtained molten steel comprising the following chemical components in percent by mass: 0.002-0.004% of C, not greater than 0.003% of S, 1.4-1.7% of Si, 0.7-0.95% of Mn, not greater than 0.03% of P, 0.015-0.035% of Sn, not greater than 0.004% of Nb, not greater than 0.004% of V, not greater than 0.005% of Ti, not greater than 0.004% of Mo, not greater than 0.03% of Cr, not greater than 0.03% of Ni, not greater than 0.03% of Cu, not greater than 0.003% of N, and the balance Fe and inevitable impurities, and 11×([Si]-1.4%)=14×([Mn]-0.7%);
2) continuously casting the molten steel obtained in step 1 into a continuous casting billet with the thickness of more than 200 mm;
3) heating the continuous casting billet obtained in step 2 to reach 1,120-1,150° C., and maintaining the temperature for more than 200 min; then carrying out multi-pass rough rolling to obtain an intermediate billet with the thickness of 40-45 mm; then carrying out multi-pass finish rolling, and coiling to obtain a hot-rolled coil with the thickness of 2.50±0.1 mm, the finishing temperature in finish rolling being (Ar1-40)±15° C., Ar1 representing the temperature for transformation from austenite to ferrite, the rolling reduction of the last pass of finish rolling being not less than 30%, the total rolling reduction of the last two passes of finish rolling being not less than 50%, and the coiling temperature being 650±20° C.; and carrying out two-stage cooling on the steel plate obtained by finishing in finish rolling before coiling, the previous-stage cooling being natural slow cooling without water cooling and lasting for 3-8 s, and the later-stage cooling being water-cooling rapid cooling;
4) carrying out uncoiling, acid pickling, rinsing, drying, cold rolling and coiling on the hot-rolled coil obtained in step 3, rather than carrying out normalizing treatment, thereby obtaining a cold hard coil with the thickness of 0.500±0.005 mm or 0.350±0.004 mm; and
5) carrying out finished product annealing on the cold hard coil obtained in step 4 in a mixed atmosphere of H2+N2 through a continuous annealing furnace, the finished product annealing temperature being 920-980° C., and the annealing time being 60±5 s; and carrying out cooling, coating and finishing on the annealed steel strip to obtain a finished product of non-oriented silicon steel.

### Claim 9 (depends on 1)

High-grade non-oriented silicon steel, prepared through the production method according to claim 1.

### Claim 10 (depends on 9)

The high-grade non-oriented silicon steel according to claim 9, wherein in a case that the thickness of the finished product of the non-oriented silicon steel is 0.500±0.005 mm, the iron loss is shown as P1.5/50≤3.8 W/kg, and the magnetic induction intensity is shown as B5000≥1.71;
or, in a case that the thickness of the finished product of the non-oriented silicon steel is 0.350±0.004 mm, the iron loss is shown as P1.5>/50≤3.3 W/kg, and the magnetic induction intensity is shown as B5000≥1.70.