# US 2023/0272525 A1 · Method of in situ ceramic coating deposition

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0272525 A1
- Document ID: US20230272525A1
- Status: Published application
- Kind: A1
- Application number: 18/143,648
- Filed: 2023-05-05
- Published: 2023-08-31
- Earliest claimed: 2020-09-29
- Assignees: Applied Materials, Inc.
- Applicants: Applied Materials, Inc.
- Inventors: Sarah Michelle BOBEK; Abdul Aziz KHAJA; Ratsamee LIMDULPAIBOON; Kwangduk Douglas LEE
- Web page: https://patentgrep.com/patent/US20230272525A1

## CPC

- C23C 16/4404: {Coatings or surface treatment on the inside of the reaction chamber or on parts thereof}
- C23C 16/30: Deposition of compounds, mixtures or solid solutions, e.g. borides, carbides, nitrides
- C23C 16/325: {Silicon carbide}
- C23C 16/401: {containing silicon}
- C23C 16/505: using radio frequency discharges
- C23C 16/56: After-treatment
- H10P 76/4085: {characterised by the processes involved to create the masks}
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- H10P: GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10

## Abstract

The present disclosure relates to a method for in situ seasoning of process chamber components, such as electrodes. The method includes depositing a silicon oxide film over the process chamber component and converting the silicon oxide film to a silicon-carbon-containing film. The silicon-carbon-containing film forms a protective film over the process chamber components and is resistant to plasma processing and/or dry etch cleaning. The coatings has high density, good emissivity control, and reduces risk of device property drift.

## Claims

### Claim 1

A method comprising:
introducing a treatment gas to a process volume of a process chamber, wherein the treatment gas comprises a silane gas and an oxygen-containing gas;
energizing the silane gas using a silane flow (sccm) to power (W) ratio of less than 0.07, wherein energizing the silane gas forms a silicon oxide (SiOx) film over a process chamber component; and
introducing a carbon-containing gas to the process volume to form a silicon-and-carbon-containing film on the process chamber component.

### Claim 2 (depends on 1)

The method of claim 1, wherein introducing a carbon-containing gas comprises converting the silicon oxide film to a silicon-and-carbon-containing film comprising silicon oxycarbide (SiOC), silicon carbide (SiC), or combination thereof.

### Claim 3 (depends on 2)

The method of claim 2, further comprising etching the silicon-and-carbon-containing film using oxygen plasma.

### Claim 4 (depends on 2)

The method of claim 2, wherein the SiOx film comprises one or more of:
an SiOx density of about 1.5 g/cc to about 2.6 g/cc, as determined by X-ray reflectometry;
an SiOx hardness of about 5 Gpa to about 8 Gpa, as determined based on ISO 14577; and
an SiOx modulus of about 50 Gpa to about 90 Gpa, as determined based on ISO 14577.

### Claim 5 (depends on 2)

The method of claim 2, wherein the silicon-and-carbon-containing film comprises one or more of:
an SiC density of about 2.0 g/cc to about 4.5 g/cc, as determined by X-ray reflectometry;
an SiC hardness of about 15 Gpa to about 30 Gpa, as determined based on ISO 14577; and
an SiC modulus of about 400 Gpa to about 515 Gpa, as determined based on ISO 14577.

### Claim 6 (depends on 1)

The method of claim 1, wherein the silane gas comprises SiH4, Si2H6, SiF4, SiH2Cl2, Si4H10, Si5H12, Tetraethyl orthosilicate (TEOS), (3-aminopropyl)triethoxysilane, triethoxymethylsilane, chloropentamethyldisilane, or combination(s) thereof.

### Claim 7 (depends on 5)

The method of claim 5, wherein the oxygen-containing gas comprises oxygen (O2), ozone (O3), water vapor (H2O), nitrous oxide, or combination(s) thereof.

### Claim 8 (depends on 1)

The method of claim 1, wherein energizing the silane gas with an RF power comprises applying an RF frequency of about 10 MHz to about 16 MHz.

### Claim 9 (depends on 7)

The method of claim 7, wherein the carbon-containing gas comprises propylene, acetylene, propane, or combination(s) thereof.

### Claim 10 (depends on 5)

The method of claim 5, wherein the carbon-containing gas includes a carrier gas, the carrier gas comprising nitrogen, hydrogen, helium, argon, or combination(s) thereof.

### Claim 11 (depends on 1)

The method of claim 1, wherein a temperature of a pedestal is about 400° C. to about 650° C. and a pressure of the process volume is about 0.05 Torr to about 12 Torr.

### Claim 12 (depends on 1)

The method of claim 1, wherein the treatment gas further comprises a dilution gas comprising nitrogen, argon, helium, or combination(s) thereof.

### Claim 13 (depends on 1)

The method of claim 1, further comprising processing a substrate in the process volume at least partially simultaneously with introducing the carbon-containing gas to the process volume such that a carbon-containing film is deposited over the substrate and the silicon oxide (SiOx) film over the process chamber component is converted to the silicon-and-carbon-containing film simultaneously.

### Claim 14

A method comprising:
introducing a treatment gas to a process volume of a process chamber, wherein the treatment gas comprises a silane gas and an oxygen-containing gas;
energizing the silane gas to form a silicon oxide (SiOx) film over a process chamber component, wherein a surface roughness (Ra) of the SiOx film is about 0.1 nm to about 0.4 nm, determined by measuring a surface roughness of a substrate after forming the SiOx film over the substrate and measuring the surface roughness based on atomic force microscopy; and
introducing a carbon-containing gas to the process volume to deposit a carbon-containing film on the process chamber component.

### Claim 15 (depends on 14)

The method of claim 14, wherein the process chamber component comprises aluminum.

### Claim 16 (depends on 14)

The method of claim 14, wherein the SiOx film comprises a refractive index (RI) at 633 nm of about 0.2 to about 0.3.

### Claim 17 (depends on 14)

The method of claim 14, wherein forming the silicon oxide film over the process chamber component comprises forming the silicon oxide film over an interior surface of orifices of a gas distribution plate using in situ chemical vapor deposition.

### Claim 18 (depends on 14)

The method of claim 14, wherein the SiOx film comprises one or more of:
a thickness of about 3 kA to about 7 kA.
an SiOx density of about 1.5 g/cc to about 2.6 g/cc, as determined by X-ray reflectometry;
an SiOx hardness of about 5 Gpa to about 8 Gpa, as determined based on ISO 14577; and
an SiOx modulus of about 50 Gpa to about 90 Gpa, as determined based on ISO 14577.

### Claim 19

A method comprising:
introducing a treatment gas to a process volume of a process chamber, wherein the treatment gas comprises a silane gas and an oxygen-containing gas;
energizing the silane gas to form a silicon oxide (SiOx) film over a surface of an electrode; and
introducing a carbon-containing gas to the process volume to form a silicon-carbon-containing film on the surface of the electrode, the silicon-carbon-containing film comprising silicon oxide (SiOx), silicon oxycarbide (SiOC), and silicon carbide (SiC).

### Claim 20 (depends on 19)

The method of claim 19, wherein the silicon-carbon-containing film is self-renewing and further comprises one or more of:
a density of about 2.0 g/cc to about 4.5 g/cc, as determined by X-ray reflectometry;
a hardness of about 15 Gpa to about 30 Gpa, as determined based on ISO 14577;
an oxygen concentration of about 65 atomic % to about 66.2 atomic %; and
a modulus of about 400 Gpa to about 515 Gpa, as determined based on ISO 14577.