# US 2023/0272502 A1 · Zinc-coated steel sheet with high resistance spot weldability

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0272502 A1
- Document ID: US20230272502A1
- Status: Published application
- Kind: A1
- Application number: 18/195,578
- Filed: 2023-05-10
- Published: 2023-08-31
- Earliest claimed: 2017-06-20
- Assignees: ArcelorMittal
- Applicants: ArcelorMittal
- Inventors: Jean-Marc PIPARD; Sebastien CREMEL; Anirban CHAKRABORTY; Damon PANAHI; Olga GIRINA; Hassan GHASSEMI-ARMAKI; Pavan CHALLA VENKATA SURYA; Yacine BENLATRECHE
- Web page: https://patentgrep.com/patent/US20230272502A1

## CPC

- C21D 9/50: for welded joints
- B23K 11/115: {by means of two electrodes placed opposite one another on both sides of the welded parts}
- B23K 11/163: {Welding of coated materials}
- B23K 31/125: {Weld quality monitoring}
- B23K 37/0408: {for planar work}
- C21D 1/20: Isothermal quenching, e.g. bainitic hardening
- C21D 1/22: Martempering
- C21D 1/76: Adjusting the composition of the atmosphere
- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0236: {Cold rolling}
- C21D 8/0247: characterised by the heat treatment
- C21D 9/46: for sheet metals
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/18: containing chromium
- C22C 38/20: with copper
- C22C 38/22: with molybdenum or tungsten
- C22C 38/24: with vanadium
- C22C 38/28: with titanium or zirconium
- C22C 38/32: with boron
- C22C 38/34: with more than 1.5% by weight of silicon
- C22C 38/38: with more than 1.5% by weight of manganese
- C22C 38/56: with more than 1.7% by weight of carbon
- C22C 38/58: with more than 1.5% by weight of manganese
- C23C 2/02: Pretreatment of the material to be coated, e.g. for coating on selected surface areas (C23C2/30 takes precedence)
- C23C 2/0222: {in a reactive atmosphere, e.g. oxidising or reducing atmosphere (C23C2/024 takes precedence)}
- C23C 2/0224: {Two or more thermal pretreatments}
- C23C 2/024: {by cleaning or etching}
- C23C 2/26: After-treatment (C23C2/14 takes precedence)
- C23C 2/40: Plates; Strips
- C23F 17/00: Multi-step processes for surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by subclass C21D or C22F or class C25 (coating for obtaining at least two superposed coatings either by methods not provided for in a single one of main groups C23C2/00 - C23C26/00, or by combinations of methods providedfor in subclasses C23C and C25D, C23C28/00)
- C25D 5/36: of iron or steel
- B23K 2101/006: {Vehicles}
- B23K 2103/04: Steel {or steel} alloys
- C21D 2211/001: Austenite
- C21D 2211/002: Bainite
- C21D 2211/008: Martensite
- C23C 2/06: Zinc or cadmium or alloys based thereon
- C25D 3/22: of zinc
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- B23K: SOLDERING OR UNSOLDERING; WELDING; CLADDING OR PLATING BY SOLDERING OR WELDING; CUTTING BY APPLYING HEAT LOCALLY, e.g. FLAME CUTTING; WORKING BY LASER BEAM
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- C23F: NON-MECHANICAL REMOVAL OF METALLIC MATERIAL FROM SURFACE (working metal by laser beams B23K26/00; desurfacing by applying flames B23K7/00; working of metal by electro-erosion B23H; producing decorative effects by removing surface material, e.g. by engraving, by etching, B44C1/22; electrolytic etching or polishing C25F); INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL; MULTI-STEP PROCESSES FOR SURFACE TREATMENT OF METALLIC MATERIAL INVOLVING AT LEAST ONE PROCESS PROVIDED FOR IN CLASS C23 AND AT LEAST ONE PROCESS COVERED BY SUBCLASS C21D OR C22F OR CLASS C25
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR

## Abstract

A method for producing a zinc or zinc-alloy coated steel sheet with a tensile strength higher than 900 MPa, for the fabrication of resistance spot welds containing in average not more than two Liquid Metal Embrittlement cracks per weld having a depth of 100 μm or more, with steps of providing a cold-rolled steel sheet, heating cold-rolled steel sheet up to a temperature T1 between 550° C. and Ac1+50° C. in a furnace zone with an atmosphere (A1) containing from 2 to 15% hydrogen by volume, so that the iron is not oxidized, then adding in the furnace atmosphere, water steam or oxygen with an injection flow rate Q higher than (0.07%/h×α), α being equal to 1 if said element is water steam or equal to 0.52 if said element is oxygen, at a temperature T≥T1, so to obtain an atmosphere (A2) with a dew point DP2 between −15° C. and the temperature Te of the iron/iron oxide equilibrium dew point, then heating the sheet from temperature T1 up to a temperature T2 between 720° C. and 1000° C. in a furnace zone under an atmosphere (A2) of nitrogen containing from 2 to 15% hydrogen and more than 0.1% CO by volume, with an oxygen partial pressure higher than 10−21 atm., wherein the duration to of heating of the sheet from temperature T1 up to the end of soaking at temperature T2 is between 100 and 500 s, soaking the sheet at T2, then cooling the sheet at a rate between 10 and 400° C./s, then coating the sheet with zinc or zinc-alloy coating.

## Claims

### Claim 1

A zinc or zinc-alloy coated steel sheet with a tensile strength higher than 900 MPa for the fabrication of resistance spot welds containing io average not more than two Liquid Metal Embrittlement cracks having a depth of 100 μm or more per weld, comprising:
a steel substrate, a nominal composition of the steel substrate containing, in weight percent:
0.07%≤C≤0.5%
0.3%≤Mn≤5%
0.010%≤Al≤1%
0.010%≤Si≤2.45%
with 0.35%≤(Si+Al)≤2.5%,
0.001%≤Cr≤1.0%
0.001%≤Mo≤0.5%
and optionally
0.005%≤Nb≤0.1%
0.005%≤V≤0.2%
0.005%≤Ti≤0.1%
0.0001%≤B≤0.004%
0.001%≤Cu≤0.5%
0.001%≤Ni≤1.0%,
a remainder being iron and unavoidable impurities from the smelting; and
a zone D100 immediately comprised between 0 and 100 micrometers under said zinc or zinc-alloy coating, wherein an average carbon content Cav(100) satisfies in said zone D100:
Cav(100)/Cnom<0.6,
Cav(100) being the average content of C in said zone D100, Cnom being the nominal C content of the steel substrate, and:
Cav(100)±(Siav(100))/32<0.21%,
Cav(100) and Siav(100) being respectively the average content of C and Si in said zone D100, expressed in weight %.

### Claim 2 (depends on 1)

The steel sheet according to claim 1 wherein:
Cav(100)+(Siav(100)/32)+(Mnav(100)/14)<0.30%,
Cav(100), Siav(100) and Mnav(100) being respectively the average content of C, Si and Mn in said zone D100, expressed in weight %.

### Claim 3 (depends on 1)

The steel sheet according to claim 1, wherein:
Cav(100)+(Siav(100)/32)+(Mnav(100)/14)−(Alav(100)/48)+(Crav(100)/11)<0.34%,
Cav(100), Siav(100), Mnav(100), Alav(100), Crav(100) being respectively the average content of C, Si, Mn, Al, Cr in said zone D100, expressed in weight %.

### Claim 4 (depends on 1)

The steel sheet according to claim 1, wherein the Mn content is not constant in said zone D100 and wherein:
dMnmin>1 μm,
dMnmin being the depth in D100 at which the Mn content is equal to the minimum value Mnmin in said zone and:
dMnmin/(Mnmin/Mnnom)>8,
Mnnom being the nominal Mn content of the steel.

### Claim 5 (depends on 1)

The steel sheet according to claim 1 wherein the Si content is not constant in said zone D100 and wherein:
dSimin>1 μm,
dSimin being the depth in D100 at which the Si content is equal to the minimum value Simin in said zone and:
dSimin/(Simin/Sinom)>4,
Sinom being the nominal Si content of the steel.

### Claim 6 (depends on 1)

The steel sheet according to claim 1 wherein the impurities include S<0.003%, P<0.02% and N<0.008%.

### Claim 7 (depends on 1)

A method for the fabrication of a resistance spot weld containing not more than two Liquid Metal Embrittlement cracks having a depth of 100 μm or more, comprising the following successive steps of:
providing at least two zinc or zinc-alloy coated steel sheets according to claim 1, a thickness of said zinc or zinc-coated steel sheets being between 0.5 and 2.5 mm; then
superposing partly at least said zinc or zinc-coated steel sheets, then
applying a force comprised between 350 and 500 daN via electrodes placed perpendicularly on outer sides of the superposed sheets; then
welding the steels sheets with an intensity I between Imin and 1.10 Imax, Imin being the minimum intensity above which pullout failure is observed when the resistance spot weld is submitted to shear tensile test, Imax being the intensity at which expulsion of liquid metal starts to be observed in resistance spot welding.

### Claim 8

A method for the fabrication of a resistance spot weld containing not more than two Liquid Metal Embrittlement cracks having a depth of 100 μm or more, comprising the following successive steps of:
providing at least two zinc or zinc-alloy coated sheets of a steel (1), with TS>900 MPa, the thickness of said zinc or zinc-alloy coated sheets being between 0.5 and 2.5 mm;
measuring C1av(100), Si1av(100), Mn1av(100), Al1av(100), Cr1av(100), designating respectively the average content of C, Si, Mn, Al, Cr in the zone D100 of the steel substrate comprised between 0 and 100 micrometers under the zinc or zinc-alloy coating; then
calculating the factor CSI1 of steel (1):
CSI1=C1av(100)+(Si1av(100)/32)+(Mn1av(100)/14)−(Al1av(100)/48)+(Cr1av(100)/11) then;
performing resistance spot welding on at least 10 welds with an intensity I1 comprised between 1 min and 1.1 Imax, Imin being the minimum intensity above which pullout failure is observed when the resistance spot weld is submitted to shear tensile test, Imax being the intensity at which expulsion of liquid metal starts to be observed in resistance spot welding; then
measuring an average number Crack1av of Liquid Metal Embrittlement cracks having a depth of 100 μm or more, from the at least 10 welds, then, if Crack1av is higher than 2,
providing a second zinc or zinc-alloy coated steel sheet (2) with TS>900 MPa, the thickness of said second zinc or zinc-alloy coated steel sheet (2 being identical to the one of steel (1), the composition of steel (2) being selected so as:
CSI2<CSI1−((Crack1av−2)/20)
with:
CSI2=C2av(100)+(Si2av(100)/32)+(Mn2av(100)/14)−(Al2av(100)/48)+(Cr2av(100)/11)
C2av(100), Si2av(100), Mn2av(100), Al2av(100), Cr2av(100) designating respectively the average content of C, Si, Mn, Al, Cr in a zone D100 of the steel (2) substrate comprised between 0 and 100 micrometers under the zinc or zinc-alloy coating; and
performing resistance spot welding on the steel sheet (2) with said intensity I1.

### Claim 9 (depends on 1)

A structural part of an automotive vehicle comprising the steel sheet according to claim 1.

### Claim 10 (depends on 1)

A method for producing a zinc or zinc-alloy coated steel sheet as recited in claim 1 comprising the successive steps of:
providing a cold-rolled steel sheet, a nominal composition of the steel sheet containing, in weight percent:
0.07%≤C≤0.5%
0.3%≤Mn≤5%
0.010%≤Al≤1%
0.010%≤Si≤2.45%
with 0.35%≤(Si+Al)≤2.5%,
0.001%≤Cr≤1.0%
0.001$≤Mo≤0.5%
and optionally
0.005%≤Nb≤0.1%
0.005%≤V≤0.2%
0.005%≤Ti≤0.1%
0.0001%≤B≤0.004%
0.001%≤Cu≤0.5%
0.001%≤Ni≤1.0%,
a remainder being iron and unavoidable impurities from smelting;
heating said cold-rolled steel sheet up to a temperature T1 between 550° C. and Ac1+50° C. in a furnace zone with an atmosphere (A1) containing from 2 to 15% hydrogen by volume, the balance being nitrogen and unavoidable impurities, so that the iron is not oxidized, then
adding in the furnace atmosphere, at least one element selected from the group consisting of water steam and oxygen with an injection flow rate Q higher than (0.07%/h×α), α being equal to 1 if said element is water steam or equal to 0.52 if said element is oxygen, at a temperature T≥T1, so to obtain an atmosphere (A2) with a dew point DP2 between −15° C. and the temperature Te of the iron/iron oxide equilibrium dew point, wherein the injection flow rate Q is the injected volume of water steam or oxygen per hour divided by the volume of the furnace between an injection location of water steam or oxygen, and an end of the furnace section heated at the soaking temperature T2;
heating the sheet from said temperature T1 up to a temperature T2 between 720° C. and 1000° C. in a furnace zone under an atmosphere (A2) of nitrogen containing from 2 to 15% hydrogen, more than 0.1% CO by volume, with an oxygen partial pressure higher than 10-21 atm., wherein the duration to of said heating of the sheet from temperature T1 up to the end of soaking at temperature T2 is between 100 and 500 s;
soaking the sheet at T2; then
cooling the sheet at a rate between 10 and 400° C./s; and then
coating the sheet with zinc or zinc-alloy coating.