# US 2023/0272497 A1 · Ultra-high strength maraging stainless steel with salt-water corrosion resistance

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0272497 A1
- Document ID: US20230272497A1
- Status: Published application
- Kind: A1
- Application number: 18/312,769
- Filed: 2023-05-05
- Published: 2023-08-31
- Earliest claimed: 2016-07-26
- Assignees: The Boeing Company; Institute of Metal Research
- Applicants: The Boeing Company; Institute of Metal Research
- Inventors: Jialong Tian; Ke Yang; Wei Wang; Yiyin Shan; Wei Yan
- Web page: https://patentgrep.com/patent/US20230272497A1

## CPC

- C21D 7/13: by hot working
- C21D 6/004: {containing Cr and Ni}
- C21D 6/005: {containing Mn}
- C21D 6/007: {containing Co}
- C21D 6/008: {containing Si}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/44: with molybdenum or tungsten
- C22C 38/50: with titanium or zirconium
- C22C 38/52: with cobalt
- C21D 2211/001: Austenite
- C21D 2211/008: Martensite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

An ultra-high strength maraging stainless steel with nominal composition (in mass) of C≤0.03%, Cr: 13.0-14.0%, Ni: 5.5-7.0%, Co: 5.5-7.5%, Mo: 3.0-5.0%, Ti: 1.9-2.5%, Si: ≤0.1%, Mn: ≤0.1%, P: ≤0.01%, S: ≤0.01%, and Fe: balance. The developed ultra-high strength maraging stainless steel combines ultra-high strength (with σb≥2000 MPa, σ0.2≥1700 MPa, δ≥8% and ψ≥40%), high toughness (KIC≥83 MPa·m1/2) and superior salt-water corrosion resistance (with pitting potential Epit≥0.15 (vs SCE)). Therefore, this steel is suitable to make structural parts that are used in harsh corrosive environments like marine environment containing chloride ions, etc.

## Claims

### Claim 1

A method for heat treatment of a stainless steel comprising:
13 to 14 wt % chromium (Cr);
5.5 to 7.0 wt % nickel (Ni);
5.5 to 7.5 wt % cobalt (Co);
3 to 5 wt % molybdenum (Mo);
1.9 to 2.5 wt % titanium (Ti); and
iron (Fe),
the method comprising:
solution treatment of the stainless steel at 1050-1150° C. for 1-2 h;
after the solution treatment, cryogenic treatment of the stainless steel in liquid nitrogen (−196° C.) for at least 5 h; and
after the cryogenic treatment, aging treatment of the stainless steel at 450-520° C. for 30 min to 16 h.

### Claim 2 (depends on 1)

The method of claim 1 wherein the solution treatment is performed at 1100° C. for 1.5 h.

### Claim 3 (depends on 1)

The method of claim 1 wherein the cryogenic treatment is performed for at least 10 h.

### Claim 4 (depends on 1)

The method of claim 1 wherein the aging treatment is performed at 480° C. for 10 h.

### Claim 5 (depends on 1)

The method of claim 1 wherein:
the solution treatment is performed at 1100° C. for 1.5 h;
the cryogenic treatment is performed for at least 10 h; and
the aging treatment is performed at 480° C. for 10 h.

### Claim 6 (depends on 1)

The method of claim 1 wherein the stainless steel comprises a carbon (C) content of at most 0.03 wt %.

### Claim 7 (depends on 1)

The method of claim 1 wherein the stainless steel comprises a silicon (Si) content of at most 0.1 wt %.

### Claim 8 (depends on 1)

The method of claim 1 wherein the stainless steel comprises a manganese (Mn) content of at most 0.1 wt %.

### Claim 9 (depends on 1)

The method of claim 1 wherein the stainless steel comprises a phosphorus (P) content of at most 0.01 wt %.

### Claim 10 (depends on 1)

The method of claim 1 wherein the stainless steel comprises a sulfur (S) content of at most 0.01 wt %.

### Claim 11 (depends on 1)

The method of claim 1 wherein the stainless steel comprises:
a carbon (C) content of at most 0.03 wt %;
a silicon (Si) content of at most 0.1 wt %;
a manganese (Mn) content of at most 0.1 wt %;
a phosphorus (P) content of at most 0.01 wt %; and
a sulfur (S) content of at most 0.01 wt %.

### Claim 12 (depends on 1)

The method of claim 1 wherein the chromium is present in the stainless steel at 13.0 to 13.1 wt %.

### Claim 13 (depends on 1)

The method of claim 1 wherein the nickel is present in the stainless steel at 6.9 to 7.0 wt %.

### Claim 14 (depends on 1)

The method of claim 1 wherein the cobalt is present in the stainless steel at 5.5 to 5.6 wt %.

### Claim 15 (depends on 1)

The method of claim 1 wherein the molybdenum is present in the stainless steel at 3.4 to 3.5 wt %.

### Claim 16 (depends on 1)

The method of claim 1 wherein the titanium is present in the stainless steel at 1.9 to 2.2 wt %.

### Claim 17 (depends on 1)

The method of claim 1 wherein:
the chromium is present in the stainless steel at 13.0 to 13.1 wt %;
the nickel is present in the stainless steel at 6.9 to 7.0 wt %;
the cobalt is present in the stainless steel at 5.5 to 5.6 wt %;
the molybdenum is present in the stainless steel at 3.4 to 3.5 wt %; and
the titanium is present in the stainless steel at 1.9 to 2.2 wt %.

### Claim 18 (depends on 1)

The method of claim 1 wherein the solution treatment of the stainless steel at 1050-1150° C. for 1-2 h is followed by air cooling to room temperature.

### Claim 19 (depends on 1)

The method of claim 1 wherein the aging treatment of the stainless steel at 450-520° C. for 30 min to 16 h is followed by air cooling.

### Claim 20

A method for heat treatment of a stainless steel comprising:
13.0 to 13.1 wt % chromium (Cr);
6.9 to 7.0 wt % nickel (Ni);
5.5 to 5.6 wt % cobalt (Co);
3.4 to 3.5 wt % molybdenum (Mo);
1.9 to 2.2 wt % titanium (Ti);
at most 0.03 wt % carbon (C);
at most 0.1 wt % silicon (Si);
at most 0.1 wt % manganese (Mn);
at most 0.01 wt % phosphorus (P);
at most 0.01 wt % sulfur (S); and
iron (Fe),
the method comprising:
solution treatment of the stainless steel at 1050-1150° C. for 1-2 h, and then air cooling to room temperature;
after the solution treatment, cryogenic treatment of the stainless steel in liquid nitrogen (−196° C.) for at least 5 h; and
after the cryogenic treatment, aging treatment of the stainless steel at 450-520° C. for 30 min to 16 h, followed by air cooling.