# US 2023/0272250 A1 · Ternary Composite Conductive Adhesive and Preparation Method therefor, Slurry and Lithium Battery

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0272250 A1
- Document ID: US20230272250A1
- Status: Published application
- Kind: A1
- Application number: 18/314,829
- Filed: 2023-05-10
- Published: 2023-08-31
- Earliest claimed: 2021-06-29
- Assignees: Fullymax Battery Co., Ltd.
- Applicants: Fullymax Battery Co., Ltd.
- Inventors: Jianxiang DENG; Changhao LIU
- Web page: https://patentgrep.com/patent/US20230272250A1

## CPC

- C09J 109/06: Copolymers with styrene
- C08K 3/04: Carbon
- C08K 3/041: {Carbon nanotubes}
- C08K 7/18: inorganic
- C09D 127/16: Homopolymers or copolymers of vinylidene fluoride
- C09J 9/02: Electrically-conducting adhesives
- C09J 11/04: inorganic
- C09J 127/16: Homopolymers or copolymers of vinylidene fluoride
- C09J 133/08: Homopolymers or copolymers of acrylic acid esters
- H01M 4/622: {being polymers}
- H01M 10/052: Li-accumulators
- C08K 2003/2203: {of lithium}
- C08K 2003/2289: {of cobalt}
- C08K 2201/001: Conductive additives
- C09J 2203/33: for batteries or fuel cells
- C09J 2301/408: additives as essential feature of the adhesive layer
- C09J 2409/00: Presence of diene rubber
- C09J 2427/00: Presence of halogenated polymer
- C09J 2433/00: Presence of (meth)acrylic polymer
- H01M 4/623: {fluorinated polymers}
- H01M 4/625: {Carbon or graphite}
- Y02E 60/10: Energy storage using batteries
- C09J: ADHESIVES; NON-MECHANICAL ASPECTS OF ADHESIVE PROCESSES IN GENERAL; ADHESIVE PROCESSES NOT PROVIDED FOR ELSEWHERE; USE OF MATERIALS AS ADHESIVES (preparation of glue or gelatine C09H)
- C08K: Use of inorganic or non-macromolecular organic substances as compounding ingredients (paints, inks, varnishes, dyes, polishes, adhesives C09)
- C09D: COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR (cosmetics A61K; processes for applying liquids or other fluent materials to surfaces, in general, B05D; staining wood B27K5/02; glazes or vitreous enamels C03C; natural resins, French polish, drying-oils, driers, turpentine, per se, C09F; polishing compositions other than French polish, ski waxes C09G; adhesives or use of materials as adhesives C09J; materials for sealing or packing joints or covers C09K3/10; materials for stopping leaks C09K3/12; processes for the electrolytic or electrophoretic production of coatings C25D)
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

A ternary composite conductive adhesive includes following items: binder, solvent, conductive agent. The conductive agent includes conductive spherical node substance, conductive fiber transition substance and tubular conductive substance.

## Claims

### Claim 1

A ternary composite conductive adhesive, including following items:
binder;
solvent; and
conductive agent, wherein the conductive agent includes conductive spherical node substance, conductive fiber transition substance and tubular conductive substance.

### Claim 2 (depends on 1)

The ternary composite conductive adhesive according to claim 1, wherein the binder is at least one of polyvinylidene fluoride, polyacrylate and butadiene styrene rubber.

### Claim 3 (depends on 1)

The ternary composite conductive adhesive according to claim 1, wherein the binder includes butadiene styrene rubber and polyacrylate.

### Claim 4 (depends on 1)

The ternary composite conductive adhesive described in claim 1, wherein the binder includes butadiene styrene rubber and polyacrylate the mass ratio of which is 0.3-0.65.

### Claim 5 (depends on 1)

The ternary composite conductive adhesive described in claim 1, wherein the solvent is organic solvent or water.

### Claim 6 (depends on 1)

The ternary composite conductive adhesive described in claim 1, wherein the conductive spherical node substance is spherical carbon black.

### Claim 7 (depends on 1)

The ternary composite conductive adhesive described in claim 1, wherein the conductive spherical node substance is at least one of furnace black, acetylene black and Ketjen black.

### Claim 8 (depends on 1)

The ternary composite conductive adhesive described in claim 1, wherein the conductive fiber transition substance is carbon fiber.

### Claim 9 (depends on 1)

The ternary composite conductive adhesive described in claim 1, its characteristic is that the tubular conductive substance is carbon nanotube.

### Claim 10 (depends on 1)

The ternary composite conductive adhesive according to claim 1, wherein the tubular conductive substance is at least one of single-walled carbon nanotube and multi-walled carbon nanotube.

### Claim 11 (depends on 1)

The ternary composite conductive adhesive according to claim 1, wherein the ternary composite conductive adhesive includes the following items in parts by mass:
binder
4-8 shares;
solvent
85-96 shares;
conductive spherical node substance
0.5-3 shares
conductive fiber transition substance
0.1-2 shares; and
tubular conductive substance
0.03-1.5 shares.

### Claim 12 (depends on 11)

The ternary composite conductive adhesive according to claim 11, wherein the binder is at least one of polyvinylidene fluoride, polyacrylate, butylbenzene rubber.

### Claim 13 (depends on 11)

The ternary composite conductive adhesive according to claim 11, wherein the binder includes butylbenzene rubber and polyacrylate.

### Claim 14 (depends on 11)

The ternary composite conductive adhesive according to claim 11, wherein the binder includes butylbenzene rubber and polyacrylate with mass ratio of 0.3-0.65.

### Claim 15 (depends on 11)

The ternary composite conductive adhesive according to claim 11, wherein the solvent is organic solvent or water.

### Claim 16 (depends on 11)

The ternary composite conductive adhesive according to claim 11, wherein the conductive spherical node substance is spherical carbon black.

### Claim 17 (depends on 11)

The ternary composite conductive adhesive according to claim 11, wherein the conductive spherical node substance is at least one of furnace black, acetylene black and Ketjen black.

### Claim 18 (depends on 11)

The ternary composite conductive adhesive according to claim 11, wherein the conductive fiber transition substance is carbon fiber.

### Claim 19 (depends on 11)

The ternary composite conductive adhesive according to claim 11, wherein the tubular conductive substance is carbon nanotube.

### Claim 20 (depends on 11)

The ternary composite conductive adhesive according to claim 11, wherein the tubular conductive substance is at least one of single-walled carbon nanotube and multi-walled carbon nanotube.

### Claim 21 (depends on 1)

A preparation method of the ternary composite conductive adhesive according to claim 1, the preparation method comprising the following steps:
performing a first mixing operation on binder and solvent so as to obtain a gel-containing solvent;
adding a tubular conductive substance to the gel-containing solvent and perform a second mixing operation;
adding a conductive fiber transition substance to the gel-containing solvent which has been subjected to the second mixing operation and perform a third mixing operation; and
adding a conductive spherical node substance to the gel-containing solvent which has been subjected to the third mixing operation and perform a fourth mixing operation.

### Claim 22 (depends on 21)

The preparation method of ternary composite conductive adhesive according to claim 21, wherein the first mixing operation is performed with a mixing speed higher than 350 r/min.

### Claim 23 (depends on 21)

According to preparation method of ternary composite conductive adhesive according to claim 21, wherein the second mixing operation is performed with a mixing speed higher than 350 r/min.

### Claim 24 (depends on 23)

According to preparation method of ternary composite conductive adhesive according to claim 23, wherein adding conductive fiber transition substance to described gel-containing solvent after second mixing and treatment for third mixing and treatment when mixing speed is higher than 350 r/min.

### Claim 25 (depends on 24)

According to preparation method of ternary composite conductive adhesive according to claim 24, wherein adding conductive spherical node substance to described gel-containing solvent after third mixing and treatment for forth mixing and treatment when mixing speed is higher than 350 r/min.

### Claim 26 (depends on 21)

A slurry, including mixed active substance and the composite conductive adhesive obtained by the preparation method according to claim 21.

### Claim 27 (depends on 26)

A battery includes the slurry according to claim 26.

### Claim 28 (depends on 27)

The battery according to claim 27, wherein a preparation method for the battery includes following steps:
mixing 4 kg polyvinylidene fluoride and 85 kg water at a stirring speed of 350 r/min;
adding 0.5 kg furnace black to a mixed solvent of polyvinylidene fluoride and described water and mix them at a stirring speed of 350 r/min;
adding 0.1 kg carbon fiber to mixed solvent of polyvinylidene fluoride and described water, mixing speed is 350 r/min;
adding 0.03 kg single-walled carbon nanotube to mixed solvent of described polyvinylidene fluoride and described water, mixing speed is 350 r/min and Ternary composite conductive adhesive is obtained;
measuring 6 kg ternary composite conductive adhesive and putting it in a 10 L double planetary mixer cylinder, firstly adding 3.5 kg lithium cobalt oxides for mixing, setting revolution of 125 HZ, and self-rotation of 3,700 RPM for 60 minutes; adding 3.5 kg lithium cobalt oxides for mixing for second time, setting revolution of 120 HZ, and self-rotation of 6,000 RPM for 150 minutes; and then using No. 200 screen mesh to filter mixed lithium cobalt oxides and ternary composite conductive adhesive to coat cathode electrodes and make cathode electrodes;
measuring 4 kg ternary composite conductive adhesive and put it in a 10 L double planetary mixer cylinder, add 3.8 kg man-made graphite to mix, setting revolution of 125 HZ and self-rotation of 5,000 RPM for 180 minutes, then using No. 200 screen mesh to filter mixed man-made graphite and the ternary composite conductive adhesive to coat anode electrodes and make anode electrodes; and
assembling the cathode electrodes, the anode electrodes, separators and electrolytes into battery, and making battery after formation and capacity classification.

### Claim 29 (depends on 27)

The battery according to claim 27, wherein a preparation method for the battery includes following steps:
mixing 6 kg polyacrylate with 90 kg N-Methyl pyrrolidone, mixing speed is 350 r/min;
adding 2 kg furnace black to mixed solvent of polyacrylate with N-Methyl pyrrolidone for mixing, mixing speed is 350 r/min;
adding 1 kg carbon fiber to mixed solvent of described polyacrylate and N-Methyl pyrrolidone for mixing, and mixing speed is 350 r/min; and
adding 0.8 kg single-walled carbon nanotube to mixed solvent of described polyacrylate and N-Methyl pyrrolidone for mixing, and mixing speed is 350 r/min and ternary composite conductive adhesive is obtained;
measuring 6 kg Ternary composite conductive adhesive and putting it in a 10 L double planetary mixer cylinder, firstly add 3.5 kg lithium cobalt oxides for mixing, setting revolution of 125 HZ, and self-rotation of 3,700 RPM for 60 minutes. Add 3.5 kg lithium cobalt oxides for mixing for second time, setting revolution of 120 HZ, and self-rotation of 6,000 RPM for 150 minutes, then using No. 200 screen mesh to filter mixed lithium cobalt oxides and Ternary composite conductive adhesive to coat cathode electrodes and make cathode electrodes;
measure 4 kg ternary composite conductive adhesive and putting it in a 10 L double planetary mixer cylinder, add 3.8 kg man-made graphite to mix, setting revolution of 125 HZ and self-rotation of 5,000 RPM for 180 minutes, then using No. 200 screen mesh to filter mixed man-made graphite and the ternary composite conductive adhesive to coat anode electrodes and make anode electrodes; and
assembling the cathode electrodes, the anode electrodes, separators and electrolytes into battery, and make battery after formation and capacity classification.

### Claim 30 (depends on 27)

The battery according to claim 27, wherein a preparation method for the battery includes the following steps:
mixing 8 kg butylbenzene rubber with 96 kg water, mixing speed is 350 r/min;
adding 3 kg furnace black to mixed solvent of butylbenzene rubber with water, mixing speed is 350 r/min;
adding 2 kg carbon fiber to mixed solvent of described butylbenzene rubber with water for mixing, and mixing speed is 350 r/min;
adding 1.5 kg single-walled carbon nanotube to mixed solvent of described butylbenzene rubber with water for mixing, and mixing speed is 350 r/min and Ternary composite conductive adhesive is obtained;
measuring 6 kg ternary composite conductive adhesive and put it in a 10 L double planetary mixer cylinder, firstly add 3.5 kg lithium cobalt oxides for mixing, set revolution of 125 HZ, and self-rotation of 3,700 RPM for 60 minutes, adding 3.5 kg lithium cobalt oxides for mixing for second time, set revolution of 120 HZ, and self-rotation of 6,000 RPM for 150 minutes, then using No. 200 screen mesh to filter mixed lithium cobalt oxides and ternary composite conductive adhesive to coat cathode electrodes and make cathode electrodes;
measuring 4 kg Ternary composite conductive adhesive and putting it in a 10 L double planetary mixer cylinder, add 3.8 kg man-made graphite to mix, setting revolution of 125 HZ and self-rotation of 5,000 RPM for 180 minutes, using No. 200 screen mesh to filter mixed man-made graphite and the ternary composite conductive adhesive to coat anode electrodes and make anode electrodes; and
assembling the cathode electrodes, the anode electrodes, separators and electrolytes into battery, and make battery after formation and capacity classification.

### Claim 31 (depends on 27)

The battery according to claim 27, wherein a preparation method for the battery includes the following steps:
using ternary composite conductive adhesive with solid content of 4.55% wt for making cathode:
mixing 1.05 kg polyacrylate, 045 kg butylbenzene rubber and 95.5 kg N-Methyl pyrrolidone and mixing speed is 350 r/min
adding 2.5 kg furnace black to mixed solvent of above-mentioned polyacrylate, butylbenzene rubber and water for mixing, mixing speed is 350 r/min;
adding 0.5 kg carbon fiber to above-mentioned polyacrylate, butylbenzene rubber and water for mixing, mixing speed is 350 r/min;
adding 0.5 kg single-walled carbon nanotube to above-mentioned polyacrylate, butylbenzene rubber and water for mixing, mixing speed is 350 r/min and Ternary composite conductive adhesive is obtained;
using ternary composite conductive adhesive with solid content of 5% wt for making anode:
mixing 1.5 kg polyacrylate and 1 kg butylbenzene rubber and 95 kg water for mixing, and mixing speed is 350 r/min;
adding 2 kg furnace black to mixed solvent of described polyacrylate, butylbenzene rubber and water, and mixing speed is 350 r/min;
adding 0.47 kg carbon fiber to mixed solvent of described polyacrylate, butylbenzene rubber and water, and mixing speed is 350 r/min;
adding 0.03 kg single-walled carbon nanotube to mixed solvent of polyacrylate, butylbenzene rubber and water, and mixing speed is 350 r/min and ternary composite conductive adhesive is obtained;
measuring 6 kg ternary composite conductive adhesive with solid content of 4.55% and putting it in a 10 L double planetary mixer cylinder, firstly adding 3.5 kg lithium cobalt oxides for mixing, setting revolution of 125 HZ, and self-rotation of 3,700 RPM for 60 minutes; adding 3.5 kg lithium cobalt oxides for mixing for second time, setting revolution of 120 HZ, and self-rotation of 6,000 RPM for 150 minutes, then using No. 200 screen mesh to filter mixed lithium cobalt oxides and ternary composite conductive adhesive to coat cathode electrodes and make cathode electrodes;
measuring 4 kg ternary composite conductive adhesive with solid content of 5% and putting it in a 10 L double planetary mixer cylinder, adding 3.8 kg man-made graphite to mix, setting revolution of 125 HZ and self-rotation of 5,000 RPM for 180 minutes, then using No. 200 screen mesh to filter mixed man-made graphite and the ternary composite conductive adhesive to coat anode electrodes and make anode electrodes; and
assembling the cathode electrodes, the anode electrodes, separators and electrolytes into battery, and make battery after formation and capacity classification.