# US 2023/0272123 A1 · Paramylon-based resin, molding material, molded body, and method for producing paramylon-based resin

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0272123 A1
- Document ID: US20230272123A1
- Status: Published application
- Kind: A1
- Application number: 18/136,931
- Filed: 2023-04-20
- Published: 2023-08-31
- Earliest claimed: 2018-07-10
- Assignees: NEC Corporation; University of Tsukuba
- Applicants: NEC Corporation; University of Tsukuba
- Inventors: Midori SHIMURA; Shukichi Tanaka; Toshie Miyamoto; Masatoshi Iji
- Web page: https://patentgrep.com/patent/US20230272123A1

## CPC

- C08B 37/0024: {beta-D-Glucans; (beta-1,3)-D-Glucans, e.g. paramylon, coriolan, sclerotan, pachyman, callose, scleroglucan, schizophyllan, laminaran, lentinan or curdlan; (beta-1,6)-D-Glucans, e.g. pustulan; (beta-1,4)-D-Glucans; (beta-1,3)(beta-1,4)-D-Glucans, e.g. lichenan; Derivatives thereof}
- A61K 36/02: Algae
- C08B: POLYSACCHARIDES; DERIVATIVES THEREOF (polysaccharides containing less than six saccharide radicals attached to each other by glycosidic linkages C07H; fermentation or enzyme-using processes C12P19/00; sugar industry C13; production of cellulose D21)
- A61K: PREPARATIONS FOR MEDICAL, DENTAL OR TOILETRY PURPOSES (devices or methods specially adapted for bringing pharmaceutical products into particular physical or administering forms A61J3/00; chemical aspects of, or use of materials for deodorisation of air, for disinfection or sterilisation, or for bandages, dressings, absorbent pads or surgical articles A61L; soap compositions C11D)

## Abstract

A paramylon-based resin having a weight-average molecular weight of paramylon in a range of 70000 to 140000, and formed by substituting hydrogen atoms of hydroxy groups of a paramylon with a long-chain component being a linear saturated aliphatic acyl group having 14 or more carbon atoms and a short-chain component being an acyl group (acetyl group or/and propionyl group) having 2 or 3 carbon atoms, wherein a degree of substitution with the long-chain component (DSLo) and a degree of substitution with the short-chain component (DSSh) satisfy the following conditional expressions (1) and (2), Izod impact strength is 5.0 kJ/m2 or more, and an MFR (melt flow rate at 210° C. and under a load of 5 kg) is 2 g/10 min or more. To provide a paramylon-based resin excellent in mechanical characteristics and thermoplasticity. 2.2≤DSLo+DSSh≤2.8 (1) 5≤DSSh/DSLo≤25 (2)

## Claims

### Claim 1

A method for producing a paramylon-based resin having a weight-average molecular weight of paramylon in a range of 70000 to 140000, and formed by substituting hydrogen atoms of hydroxy groups of a paramylon with a long-chain component being a linear saturated aliphatic acyl group having 14 or more carbon atoms and a short-chain component being an acyl group (acetyl group or/and propionyl group) having 2 or 3 carbon atoms,
wherein a degree of substitution with the long-chain component (DSLo) and a degree of substitution with the short-chain component (DSSh) satisfy the following conditional expressions (1) and (2):
2.2≤DSLo+DSSh≤2.8 (1)
5≤DSSh/DSLo≤25 (2),
Izod impact strength is 5.0 kJ/m2 or more, and
an MFR (melt flow rate at 210° C. and under a load of 5 kg) is 2 g/10 min or more;
said method comprising:
acylating hydroxy groups of a paramylon by reacting
the paramylon having a weight average molecular weight of 70000 to 140000 and dispersed in a solvent with
acetyl chloride or/and propionyl chloride, and
a long-chain reactant being an acid chloride of a long-chain fatty acid and comprising the long-chain component,
in the presence of the acid trapping component and under warming; and
separating an acylated paramylon obtained in the acylating from the solvent.

### Claim 2 (depends on 1)

The method for producing the paramylon-based resin according to claim 1, wherein the solvent is at least one selected from the group consisting of water, acetic acid, dioxane, pyridine, N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, and dimethyl sulfoxide.

### Claim 3 (depends on 1)

The method for producing the paramylon-based resin according to claim 1, wherein the acid trapping component comprises triethylamine or pyridine.

### Claim 4 (depends on 1)