# US 2023/0265947 A1 · Seamless steel pipe and method of manufacture thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0265947 A1
- Document ID: US20230265947A1
- Status: Published application
- Kind: A1
- Application number: 18/020,458
- Filed: 2021-07-21
- Published: 2023-08-24
- Earliest claimed: 2020-08-19
- Assignees: Jfe Steel Corporation
- Applicants: Jfe Steel Corporation
- Inventors: Shunsuke SASAKI; Ryosuke TACHI; Hiroyuki YAMASAKI; Hiroyuki FUKUDA
- Web page: https://patentgrep.com/patent/US20230265947A1

## CPC

- C21D 8/10: during manufacturing of tubular bodies
- F16L 9/02: of metal (F16L9/16 - F16L9/22 take precedence)
- B21B 19/04: Rolling basic material of solid, i.e. non-hollow, structure; Piercing {, e.g. rotary piercing mills}
- C21D 1/26: Methods of annealing
- C21D 1/28: Normalising
- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C21D 9/08: for tubular bodies or pipes
- C22C 38/001: {containing N}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/18: containing chromium
- C22C 38/22: with molybdenum or tungsten
- C22C 38/40: with nickel
- C22C 38/44: with molybdenum or tungsten
- C22C 38/54: with boron
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- F16L: PIPES; JOINTS OR FITTINGS FOR PIPES; SUPPORTS FOR PIPES, CABLES OR PROTECTIVE TUBING; MEANS FOR THERMAL INSULATION IN GENERAL
- B21B: ROLLING OF METAL (auxiliary operations used in connection with metal-working operations covered in B21, see B21C; bending by rolling B21D; manufacture of particular objects, e.g. screws, wheels, rings, barrels, balls, by rolling B21H; pressure welding by means of a rolling mill B23K20/04)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

A seamless steel pipe has a t/Dout of 0.05 to 0.40, where t is a wall thickness (mm) of the seamless steel pipe, and Dout is an outside diameter (mm) of the seamless steel pipe. The seamless steel pipe has a maximum depth dmax (mm)≤0.350 mm for defects in an inner surface of the steel pipe on a cross section perpendicular to a pipe axis. The seamless steel pipe has an average defect depth dave (mm)≤0.200 mm for defects having a depth of 0.050 mm or more in the inner surface of the steel pipe. The seamless steel pipe, per millimeter of an inner circumferential length of the pipe, has at most 30 defects having a depth of 0.050 mm or more in the inner surface of the steel pipe.

## Claims

### Claim 1

A seamless steel pipe having:
a t/Dout of 0.05 to 0.40, where t is a wall thickness (mm) of the seamless steel pipe, and Dout is an outside diameter (mm) of the seamless steel pipe,
a maximum depth dmax (mm)≤0.350 for defects in an inner surface of the seamless steel pipe in a cross section of the seamless steel pipe perpendicular to a pipe axis,
an average defect depth dave (mm)≤0.200 for defects having a depth of 0.050 mm or more in the inner surface of the seamless steel pipe,
per millimeter of an inner circumferential length of the seamless steel pipe, at most 30 defects having a depth of 0.050 mm or more in the inner surface of the seamless steel pipe.

### Claim 2 (depends on 1)

The seamless steel pipe according to claim 1, having a microstructure comprising:
ferrite grains having an average grain size of 15 μm or less, or
prior austenite grains having an average grain size of 15 μm or more.

### Claim 3 (depends on 1)

The seamless steel pipe according to claim 1, having:
a chemical composition comprising, in mass %:
C: 0.05 to 0.45%,
Si: 0.05 to 0.45%,
Mn: 0.05 to 1.2%, and
Cr: less than 4.5%, and
a microstructure comprising ferrite grains having an average grain size of 15 μm or less.

### Claim 4 (depends on 1)

The seamless steel pipe according to claim 1, having:
a chemical composition comprising, in mass %:
C: 0.05 to 0.45%,
Si: 0.05 to 0.45%,
Mn: 0.05 to 1.2%, and
Cr: 4.5% to 9.5%, and
a microstructure comprising prior austenite grains having an average grain size of 15 μm or more.

### Claim 5 (depends on 3)

The seamless steel pipe according to claim 3, wherein the chemical composition further comprises, in mass %, one or more selected from the group consisting of:
Ni: 0.5% or less,
Mo: 1.5% or less,
W: 2.5% or less,
N: 0.10% or less, and
B: 0.010% or less.

### Claim 6 (depends on 4)

The seamless steel pipe according to claim 4, wherein the chemical composition further comprises, in mass %, one or more selected from selected from the group consisting of:
Ni: 0.5% or less,
Mo: 1.5% or less,
W: 2.5% or less,
N: 0.10% or less, and
B: 0.010% or less.

### Claim 7 (depends on 1)

A method for manufacturing the seamless steel pipe of claim 1, the method comprising:
subjecting a steel billet to pierce rolling, wall-thickness reduction and stretch rolling to form a steel pipe; and
sizing the steep pipe according to the following formula (1):
(Dini−Dout)2×t02×GD2≤9980 (1),
where:
GD is an average grain size (mm) of austenite before sizing,
Dini is a steel pipe outside diameter (mm) before sizing,
Dout is a steel pipe outside diameter (mm) after sizing, and
t0 is a wall thickness (mm) before sizing,
thereby producing the seamless steel pipe of claim 1.

### Claim 8

(canceled)

### Claim 9 (depends on 2)

A method for manufacturing the seamless steel pipe of claim 2, the method comprising:
subjecting a steel billet to pierce rolling, wall-thickness reduction and stretch rolling to form a steel pipe; and
sizing the steep pipe according to the following formula (1):
(Dini−Dout)2×t02×GD2≤9980 (1),
where:
GD is an average grain size (mm) of austenite before sizing,
Dini is a steel pipe outside diameter (mm) before sizing,
Dout is a steel pipe outside diameter (mm) after sizing, and
t0 is a wall thickness (mm) before sizing,
to produce the seamless steel pipe of claim 2.

### Claim 10 (depends on 3)

A method for manufacturing the seamless steel pipe of claim 3, the method comprising:
subjecting a steel billet to pierce rolling, wall-thickness reduction and stretch rolling to form a steel pipe; and
sizing the steep pipe according to the following formula (1):
(Dini−Dout)2×t02×GD2≤9980 (1),
where:
GD is an average grain size (mm) of austenite before sizing,
Dini is a steel pipe outside diameter (mm) before sizing,
Dout is a steel pipe outside diameter (mm) after sizing, and
t0 is a wall thickness (mm) before sizing,
to produce the seamless steel pipe of claim 3.

### Claim 11 (depends on 4)

A method for manufacturing the seamless steel pipe of claim 4, the method comprising:
subjecting a steel billet to pierce rolling, wall-thickness reduction and stretch rolling to form a steel pipe; and
sizing the steep pipe according to the following formula (1):
(Dini−Dout)2×t02×GD2≤9980 (1),
where:
GD is an average grain size (mm) of austenite before sizing,
Dini is a steel pipe outside diameter (mm) before sizing,
Dout is a steel pipe outside diameter (mm) after sizing, and
t0 is a wall thickness (mm) before sizing,
to produce the seamless steel pipe of claim 4.

### Claim 12 (depends on 5)

A method for manufacturing the seamless steel pipe of claim 5, the method comprising:
subjecting a steel billet to pierce rolling, wall-thickness reduction and stretch rolling to form a steel pipe; and
sizing the steep pipe according to the following formula (1):
(Dini−Dout)2×t02×GD2≤9980 (1),
where:
GD is an average grain size (mm) of austenite before sizing,
Dini is a steel pipe outside diameter (mm) before sizing,
Dout is a steel pipe outside diameter (mm) after sizing, and
t0 is a wall thickness (mm) before sizing,
to produce the seamless steel pipe of claim 5.

### Claim 13 (depends on 6)

A method for manufacturing the seamless steel pipe of claim 6, the method comprising:
subjecting a steel billet to pierce rolling, wall-thickness reduction and stretch rolling to form a steel pipe; and
sizing the steep pipe according to the following formula (1):
(Dini−Dout)2×t02×GD2≤9980 (1),
where:
GD is an average grain size (mm) of austenite before sizing,
Dini is a steel pipe outside diameter (mm) before sizing,
Dout is a steel pipe outside diameter (mm) after sizing, and
t0 is a wall thickness (mm) before sizing,
to produce the seamless steel pipe of claim 6.

### Claim 14 (depends on 7)

The method according to claim 7, further comprising:
subjecting the sized steel pipe to a heat treatment at a heating temperature in a range of 850 to 1,150° C. with at least 10 minutes of soaking retention time.

### Claim 15 (depends on 9)

The method according to claim 9, further comprising:
subjecting the sized steel pipe to a heat treatment at a heating temperature in a range of 850 to 1,150° C. with at least 10 minutes of soaking retention time.

### Claim 16 (depends on 10)

The method according to claim 10, further comprising:
subjecting the sized steel pipe to a heat treatment at a heating temperature in a range of 850 to 1,150° C. with at least 10 minutes of soaking retention time.

### Claim 17 (depends on 11)

The method according to claim 11, further comprising:
subjecting the sized steel pipe to a heat treatment at a heating temperature in a range of 850 to 1,150° C. with at least 10 minutes of soaking retention time.

### Claim 18 (depends on 12)

The method according to claim 12, further comprising:
subjecting the sized steel pipe to a heat treatment at a heating temperature in a range of 850 to 1,150° C. with at least 10 minutes of soaking retention time.

### Claim 19 (depends on 13)

The method according to claim 13, further comprising:
subjecting the sized steel pipe to a heat treatment at a heating temperature in a range of 850 to 1,150° C. with at least 10 minutes of soaking retention time.