# US 2023/0202856 A1 · Process for manufacturing high-purity magnesium oxide

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0202856 A1
- Document ID: US20230202856A1
- Status: Published application
- Kind: A1
- Application number: 17/919,336
- Filed: 2021-04-20
- Published: 2023-06-29
- Earliest claimed: 2020-04-20
- Assignees: Purac Biochem B.V.
- Applicants: Purac Biochem B.V.
- Inventors: Fesia Lestari LAKSMANA; Raymon FREDIANSYAH
- Web page: https://patentgrep.com/patent/US20230202856A1

## CPC

- C01F 5/10: by thermal decomposition of magnesium chloride with water vapour
- C07C 51/02: from salts of carboxylic acids
- C07C 59/08: Lactic acid
- C12P 7/56: Lactic acid
- C01P 2004/61: Micrometer sized, i.e. from 1-100 micrometer
- C01P 2004/62: Submicrometer sized, i.e. from 0.1-1 micrometer
- Y02P 20/10: Process efficiency
- C01F: COMPOUNDS OF THE METALS BERYLLIUM, MAGNESIUM, ALUMINIUM, CALCIUM, STRONTIUM, BARIUM, RADIUM, THORIUM, OR OF THE RARE-EARTH METALS (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts of peroxyacids C01B15/00; sulfides or polysulfides of magnesium, calcium, strontium, or barium C01B17/42; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds other than ammonia or cyanogen containing nitrogen and non-metals and optionally metals C01B21/082; amides or imides of silicon C01B21/087}; metal {imides or} amides C01B21/092, {C01B21/0923}; nitrites C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; compounds having molecular sieve properties but not having base-exchange properties C01B37/00; compounds having molecular sieve and base-exchange properties, e.g. crystalline zeolites, C01B39/00; cyanides C01C3/08; salts of cyanic acid C01C3/14; salts of cyanamide C01C3/16; thiocyanates C01C3/20; {double sulfates of magnesium with sodium or potassium C01D5/12; with other alkali metals C01D15/00, C01D17/00})
- C07C: ACYCLIC OR CARBOCYCLIC COMPOUNDS
- C12P: FERMENTATION OR ENZYME-USING PROCESSES TO SYNTHESISE A DESIRED CHEMICAL COMPOUND OR COMPOSITION OR TO SEPARATE OPTICAL ISOMERS FROM A RACEMIC MIXTURE {(brewing of beer C12C; producing vinegar C12J; producing specific peptides or proteins C07K; producing enzymes C12N9/00; DNA or RNA concerning genetic engineering, vectors, e.g. plasmids, or their isolation, preparation or purification C12N15/00; measuring or testing processes involving enzymes or microorganisms C12Q; measuring or testing processes involving nucleic acid amplification reactions C12Q1/6844; fermentation processes to form a food composition, A21 or A23; compounds in general, see the relevant compound class, e.g. C01, C07)}
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

A process for converting magnesium chloride into magnesium oxide having the steps of: subjecting a magnesium chloride solution to a spray drying step in a spray-drying apparatus at a temperature of 300-475° C., resulting in the formation of a spray-dried product having 10-80 wt. % magnesium oxide and 20-90 wt. % of the total of magnesium hydroxychloride and magnesium chloride, subjecting the product of the spray drying step to a roasting step in a roaster at a temperature of 600-900° C. in the presence of water, resulting in the formation of a product having at least 98 wt. % of MgO, and less than 2 wt. % of the total of magnesium hydroxychloride and magnesium chloride, wherein the percentages of MgO, magnesium hydroxychloride and magnesium chloride, are calculated on the total of MgO, magnesium hydroxychloride and magnesium chloride.

## Claims

### Claim 1

A process for converting magnesium chloride into magnesium oxide comprising the steps of
subjecting a magnesium chloride solution to a spray drying step at a temperature in the range of 300-475° C., resulting in the formation of a spray-dried product comprising 10-80 wt. % magnesium oxide and 20-90 wt. % of the total of magnesium hydroxychloride and magnesium chloride,
subjecting the product of the spray drying step to a roasting step in a roaster at a temperature of 600-900° C. in the presence of water, resulting in the formation of a product comprising at least 98 wt. % of MgO, and less than 2 wt. % of the total of magnesium hydroxychloride and magnesium chloride, wherein the percentages of MgO, magnesium hydroxychloride and magnesium chloride, are calculated on the total of MgO, magnesium hydroxychloride and magnesium chloride.

### Claim 2 (depends on 1)

The process according to claim 1, wherein the first step encompasses subjecting a magnesium chloride solution to a spray drying step in a spray-drying apparatus, at a temperature in the range of 350-450° C., resulting in the formation of a spray-dried product comprising 30-80 wt. % magnesium oxide and 20-70 wt. % of the total of magnesium hydroxychloride and magnesium chloride.

### Claim 3 (depends on 1)

The process according to claim 1, wherein the magnesium chloride solution provided to the spray-drying step has a magnesium chloride concentration of 5-48 wt. %.

### Claim 4 (depends on 1)

The process according to claim 1, wherein spray-drying is carried out at a temperature in the range of 375 to 450° C.

### Claim 5 (depends on 1)

The process according to claim 1, wherein the product from the spray-drying step comprises 40-80 wt. % magnesium oxide and 20-60 wt. % of the total of magnesium hydroxychloride and magnesium chloride, all calculated on total solids content.

### Claim 6 (depends on 1)

The process according to claim 1, wherein the temperature in the roaster is in the range of 700° C. to 850° C.

### Claim 7 (depends on 1)

The process according to claim 1, wherein the product of the roasting step comprises at least 98.5 wt. % of MgO, and less than 1.5 wt. % of the total of magnesium hydroxychloride and magnesium chloride, calculated on the total of MgO, magnesium hydroxychloride and magnesium chloride, or the product of the roasting step comprises at least 98 wt. % of MgO and less than 2 wt. % of the total of magnesium hydroxychloride and magnesium chloride, calculated on total solid product.

### Claim 8

A magnesium oxide product, wherein:
it comprises at least 98 wt. % of MgO, and less than 2 wt. % of the total of magnesium hydroxychloride and magnesium chloride, all percentages calculated on total solid product,
it has a D50 in the range of 0.5 to 20 micron,
it has a citric acid reactivity in the range of 75-400 s.

### Claim 9 (depends on 8)

A process for the manufacture of carboxylic acid, comprising the step of
providing a magnesium oxide of claim 8, or a magnesium oxide obtainable or obtained by a process for converting magnesium chloride into magnesium oxide comprising the steps of
subjecting a magnesium chloride solution to a spray drying step at a temperature in the range of 300-475° C., resulting in the formation of a spray-dried product comprising 10-80 wt. % magnesium oxide and 20-90 wt. % of the total of magnesium hydroxychloride and magnesium chloride,
subjecting the product of the spray drying step to a roasting step in a roaster at a temperature of 600-900° C. in the presence of water, resulting in the formation of a product comprising at least 98 wt. % of MgO, and less than 2 wt. % of the total of magnesium hydroxychloride and magnesium chloride, wherein the percentages of MgO, magnesium hydroxychloride and magnesium chloride, are calculated on the total of MgO, magnesium hydroxychloride and magnesium chloride, as neutralizing agent to a fermentation step, as such or after a conversion step into magnesium hydroxide by reacting the magnesium oxide product with water, which fermentation step comprises the steps of fermenting a carbon source by means of a micro-organism in a fermentation medium to form carboxylic acid, with the carboxylic acid being converted at least in part by the neutralizing agent, resulting in the formation of a magnesium carboxylate salt.

### Claim 10 (depends on 9)

The process according to claim 9, which comprises the further steps of
subjecting the magnesium carboxylate to an acidification step wherein the magnesium carboxylate is contacted with HCl in an aqueous environment to form an aqueous mixture comprising carboxylic acid and magnesium chloride,
subjecting the aqueous mixture comprising carboxylic acid and magnesium chloride to a separation step, to form an effluent comprising carboxylic acid and an aqueous magnesium chloride solution.

### Claim 11 (depends on 10)

The process according to claim 10, wherein after the separation step the carboxylic acid is subjected to a purification step.

### Claim 12 (depends on 10)

The process according to claim 10, wherein a biomass removal step is carried out between the fermentation step and the acidification step.

### Claim 13 (depends on 10)

The process according to claim 10, wherein at least part of the HCl produced in one or more of the spray drying step and the roasting step is provided to the acidification step.

### Claim 14 (depends on 9)

The process according to claim 9, wherein the carboxylic acid is a mono-, di- or tri-carboxylic acid comprising at least 2, but no more than 8 carbon atoms.

### Claim 15 (depends on 10)

A method according to claim 10, wherein the carboxylic acid is lactic acid, which is subsequently converted into lactide or polylactide.

### Claim 16

A process for manufacturing a carboxylic acid comprising the steps of
subjecting a carbon source to a fermentation step to form a carboxylic acid, which fermentation step comprises the steps of fermenting a carbon source by means of a micro-organism in a fermentation broth to form carboxylic acid and neutralizing at least part of the carboxylic acid by adding a magnesium base selected from magnesium oxide and magnesium hydroxide, thereby obtaining a magnesium carboxylate,
subjecting the magnesium carboxylate to an acidification step, wherein the magnesium carboxylate is contacted with HCl in an aqueous environment to form an aqueous mixture comprising carboxylic acid and magnesium chloride,
subjecting the aqueous mixture comprising carboxylic acid and magnesium chloride to a separation step, resulting in a carboxylic acid and a magnesium chloride solution separated therefrom,
subjecting the magnesium chloride solution to a spray drying step at a temperature in the range of 300-475° C., resulting in the formation of a spray-dried product comprising 10-80 wt. % magnesium oxide and 20-90 wt. % of the total of magnesium hydroxychloride and magnesium chloride,
subjecting the product of the spray drying step to a roasting step in a roaster at a temperature of 600-900° C. in the presence of water, resulting in the formation of a product comprising at least 98 wt. % of MgO, and less than 2 wt. % of the total of magnesium hydroxychloride and magnesium chloride, wherein the percentages of MgO, magnesium hydroxychloride and magnesium chloride, are calculated on the total of MgO, magnesium hydroxychloride and magnesium chloride.