# US 2023/0151474 A1 · Metal rings formed from beryllium-copper alloys

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0151474 A1
- Document ID: US20230151474A1
- Status: Published application
- Kind: A1
- Application number: 18/157,539
- Filed: 2023-01-20
- Published: 2023-05-18
- Earliest claimed: 2017-11-17
- Assignees: Materion Corporation
- Applicants: Materion Corporation
- Inventors: Jeffrey M. Schirm; Christopher W. Damschroder; Edward B. Longenberger; Jeffrey A. McBride
- Web page: https://patentgrep.com/patent/US20230151474A1

## CPC

- C22F 1/08: of copper or alloys based thereon
- B21K 1/761: {rings}
- C21D 9/40: for rings; for bearing races
- C22C 9/00: Alloys based on copper
- C22F 1/002: {by rapid cooling or quenching; cooling agents used therefor}
- F16C 2220/44: by rolling
- F16C 2300/14: Large applications, e.g. bearings having an inner diameter exceeding 500 mm
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)
- B21K: MAKING FORGED OR PRESSED METAL PRODUCTS, e.g. HORSE-SHOES, RIVETS, BOLTS OR WHEELS (making particular articles by working sheet metal without essentially removing material B21D; processing wire B21F; making pins, needles or nails B21G; making particular articles by rolling B21H; forging machines, pressing machines, hammering machines, in general B21J; making chains B21L; plating B23K)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- F16C: SHAFTS; FLEXIBLE SHAFTS; ELEMENTS OR CRANKSHAFT MECHANISMS; ROTARY BODIES OTHER THAN GEARING ELEMENTS; BEARINGS

## Abstract

Processes are disclosed for forming beryllium-copper metal rings having a fine and uniform grain structure. A raw BeCu casting is pre-forged and turned to form a BeCu billet. The BeCu billet is subjected to various heat treatment and cooling cycles to obtain/maintain combinations of advantageous material properties. Generally, the BeCu billet is preheated, hot worked via forging, heated again, hot worked again via ring rolling followed by air cooling, solution annealed followed by quenching, and heated a final time followed by air cooling.

## Claims

### Claim 1

A process for making a metal ring from a BeCu alloy, comprising:
preheating a BeCu alloy billet at a temperature of about 800° C. to about 850° C., wherein the BeCu alloy comprises about 1.6 wt % to about 2.0 wt % beryllium;
forging the billet into a ring-shaped preform at a temperature of about 750° C. to about 850° C.;
soaking the preform at a temperature of about 815° C. to about 835° C.;
ring rolling the preform at a temperature of about 750° C. to about 850° C. to form a ring having a wall thickness, wherein the ring rolling reduces the wall thickness by at least 50%;
solution annealing the ring at a temperature of about 780° C. to about 800° C., immediately followed by quenching the ring; and
heat treating the ring at a temperature of about 385° C. to about 400° C.

### Claim 2 (depends on 1)

The process of claim 1, wherein the preheating occurs for a period of at least 8 hours.

### Claim 3 (depends on 1)

The process of claim 1, wherein the soaking occurs for a minimum period of 2 hours.

### Claim 4 (depends on 3)

The process of claim 3, wherein the soaking is performed for a period of at least 8 hours if the preform has cooled to a temperature of about 600° C. or less.

### Claim 5 (depends on 1)

The process of claim 1, wherein the solution annealing occurs for a period of at least 1.5 hours.

### Claim 6 (depends on 1)

The process of claim 1, wherein the heat treating occurs for a period of about 3 hours.

### Claim 7 (depends on 6)

The process of claim 6, further comprising starting the about 3 hour period at a temperature of about 393° C., raising the temperature to about 400° C., and heat treating the ring at the about 400° C. temperature for the remaining period of time.

### Claim 8 (depends on 1)

The process of claim 1, wherein the preheating and soaking are each performed at a temperature of about 820° C.

### Claim 9 (depends on 1)

The process of claim 1, wherein the ring rolling reduces the wall thickness by at least 70%.

### Claim 10 (depends on 1)

The process of claim 1, wherein the solution annealing is performed for a period of about 30 minutes for approximately every 25 mm of wall thickness of the ring.

### Claim 11 (depends on 1)

The process of claim 1, further comprising air cooling the ring after both the ring rolling and the heat treating.

### Claim at position 12

-18. (canceled)

### Claim 19

A process for making a metal ring comprising:
providing a billet made from a BeCu alloy comprising about 1.6 wt % to about 2.0 wt % beryllium;
preheating the billet at a temperature of about 800° C. to about 850° C. for a period of at least 8 hours;
forming a ring-shaped preform from the billet at a temperature of about 750° C. to about 850° C.;
soaking the preform at a temperature of about 815° C. to about 835° C. for a period of about 2 hours to about 8 hours;
ring rolling the preform at a temperature of about 750° C. to about 850° C. until the preform has a substantially uniform wall thickness, followed by air cooling;
solution annealing the preform at a temperature of about 780° C. to about 800° C. for a period of at least 1.5 hours, immediately followed by quenching in a quench medium;
heat treating the preform at a temperature of about 385° C. to about 400° C. for a period of about 3 hours, followed by air cooling; and,
mechanically machining the preform to form the metal ring having a desired shape.

### Claim 20

(canceled)

### Claim 21 (depends on 19)

The process of claim 19, wherein the BeCu alloy billet comprises from about 1.8 wt % to about 2.0 wt % beryllium.

### Claim 22 (depends on 19)

The process of claim 19, wherein the BeCu alloy billet further comprises from about 0.2 wt % to about 0.3 wt % cobalt.

### Claim 23 (depends on 19)

The process of claim 19, wherein the BeCu alloy billet comprises:
about 1.8 wt % to about 2.0 wt % beryllium;
an amount of nickel, cobalt, and optionally iron such that the sum of (nickel+cobalt) is about 0.2 wt % or higher, and the sum of (nickel+cobalt+iron) is about 0.6 wt % or less;
about 0.2 wt % to about 0.6 wt % lead; and
balance copper.

### Claim 24 (depends on 1)

The process of claim 1, wherein the BeCu alloy billet comprises from about 1.8 wt % to about 2.0 wt % beryllium.

### Claim 25 (depends on 1)

The process of claim 1, wherein the BeCu alloy billet further comprises from about 0.2 wt % to about 0.3 wt % cobalt.

### Claim 26 (depends on 1)

The process of claim 1, wherein the BeCu alloy billet comprises:
about 1.8 wt % to about 2.0 wt % beryllium;
an amount of nickel, cobalt, and optionally iron such that the sum of (nickel+cobalt) is about 0.2 wt % or higher, and the sum of (nickel+cobalt+iron) is about 0.6 wt % or less;
about 0.2 wt % to about 0.6 wt % lead; and
balance copper.

### Claim 27 (depends on 1)

The process of claim 1, wherein the BeCu alloy billet comprises:
about 1.6 wt % to about 2.0 wt % beryllium;
about 0.2 wt % to about 0.3 wt % cobalt; and
balance copper.

### Claim 28 (depends on 1)

The process of claim 1, wherein the BeCu alloy billet comprises:
about 1.8 wt % to about 2.0 wt % beryllium;
an amount of nickel, cobalt, and optionally iron such that the sum of (nickel+cobalt) is about 0.2 wt % or higher, and the sum of (nickel+cobalt+iron) is about 0.6 wt % or less; and
balance copper.