# US 2023/0105669 A1 · Dip Molding Emulsion, Method of Producing Glove, and Glove

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0105669 A1
- Document ID: US20230105669A1
- Status: Published application
- Kind: A1
- Application number: 17/969,755
- Filed: 2022-10-20
- Published: 2023-04-06
- Earliest claimed: 2018-04-06
- Assignees: Midori Anzen Co., Ltd.
- Applicants: Midori Anzen Co., Ltd.
- Inventors: Norihide Enomoto; Taichi Ogawa; Kaname Shibata; Junji Shibasaki
- Web page: https://patentgrep.com/patent/US20230105669A1

## CPC

- C08L 9/02: Copolymers with acrylonitrile
- C09D 109/02: Copolymers with acrylonitrile
- A41D 19/0062: {made of one layer of material}
- A61B 42/10: Surgical gloves
- B29C 41/14: Dipping a core {(B29C41/10 takes precedence)}
- B29C 41/46: Heating or cooling
- B29C 41/52: Measuring, controlling or regulating
- C08J 3/248: {Measuring crosslinking reactions}
- C08J 3/26: of latex
- C08J 5/02: Direct processing of dispersions, e.g. latex, to articles
- C08J 5/18: Manufacture of films or sheets
- C08K 3/22: of metals
- C08L 63/00: Compositions of epoxy resins; Compositions of derivatives of epoxy resins
- C09D 109/04: Latex
- A41D 19/0055: {Plastic or rubber gloves}
- A41D 2500/54: in coated form
- B29K 2021/00: Use of unspecified rubbers as moulding material
- B29K 2033/18: Polymers of nitriles
- B29K 2105/24: crosslinked or vulcanised
- B29L 2031/4864: {Gloves}
- C08J 2300/26: Elastomers
- C08J 2309/02: Copolymers with acrylonitrile
- C08J 2309/04: Latex
- C08J 2313/02: Latex
- C08K 2003/2241: {Titanium dioxide}
- C08K 2003/2296: {of zinc}
- C08K 2201/014: Additives containing two or more different additives of the same subgroup in C08K
- C08L: COMPOSITIONS OF MACROMOLECULAR COMPOUNDS (compositions based on polymerisable monomers C08F, C08G; artificial filaments or fibres D01F; textile treating compositions D06)
- C09D: COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR (cosmetics A61K; processes for applying liquids or other fluent materials to surfaces, in general, B05D; staining wood B27K5/02; glazes or vitreous enamels C03C; natural resins, French polish, drying-oils, driers, turpentine, per se, C09F; polishing compositions other than French polish, ski waxes C09G; adhesives or use of materials as adhesives C09J; materials for sealing or packing joints or covers C09K3/10; materials for stopping leaks C09K3/12; processes for the electrolytic or electrophoretic production of coatings C25D)
- A41D: OUTERWEAR; PROTECTIVE GARMENTS; ACCESSORIES
- A61B: DIAGNOSIS; SURGERY; IDENTIFICATION (usefulness limited to only animals A61D)
- B29C: SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING (making preforms B29B11/00; making laminated products by combining previously unconnected layers which become one product whose layers will remain together B32B37/00 - B32B41/00)
- C08J: WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H (working, e.g. shaping, of plastics B29)
- C08K: Use of inorganic or non-macromolecular organic substances as compounding ingredients (paints, inks, varnishes, dyes, polishes, adhesives C09)
- B29K: INDEXING SCHEME ASSOCIATED WITH SUBCLASSES B29B, B29C OR B29D, RELATING TO MOULDING MATERIALS OR TO MATERIALS FOR {MOULDS, } REINFORCEMENTS, FILLERS OR PREFORMED PARTS, e.g. INSERTS
- B29L: INDEXING SCHEME ASSOCIATED WITH SUBCLASS B29C, RELATING TO PARTICULAR ARTICLES

## Abstract

Provided is a dip molding emulsion including, at least: an elastomer that contains a (meth)acrylonitrile-derived structural unit, an unsaturated carboxylic acid-derived structural unit, and a butadiene-derived structural unit in a polymer main chain; an epoxy crosslinking agent; water; and a pH modifier, in which dip molding composition the elastomer contains the (meth)acrylonitrile-derived structural unit in an amount of 20% by weight to 40% by weight, the unsaturated carboxylic acid-derived structural unit in an amount of 1% by weight to 10% by weight, and the butadiene-derived structural unit in an amount of 50% by weight to 75% by weight, and the epoxy crosslinking agent includes an epoxy crosslinking agent containing an epoxy compound having three or more epoxy groups in one molecule and has a dissolution rate in water of 10% to 70% as determined by a specific measurement method.

## Claims

### Claim 1

A dip molding emulsion comprising, at least:
an elastomer that contains a (meth)acrylonitrile-derived structural unit, an unsaturated carboxylic acid-derived structural unit, and a butadiene-derived structural unit in a polymer main chain;
an epoxy crosslinking agent;
water; and
a pH modifier,
wherein
the elastomer contains the (meth)acrylonitrile-derived structural unit in an amount of 20% by weight to 40% by weight, the unsaturated carboxylic acid-derived structural unit in an amount of 1% by weight to 10% by weight, and the butadiene-derived structural unit in an amount of 50% by weight to 75% by weight,
the epoxy crosslinking agent consists of an epoxy compound having a basic skeleton that contains plural glycidyl ether groups and alicyclic, aliphatic, or aromatic hydrocarbons in one molecule,
the epoxy crosslinking agent has an average number of epoxy groups per molecule of greater than 2.0, and
the epoxy crosslinking agent has a dissolution rate in water of 10% to 70% as determined by the following measurement method:
Method of measuring the dissolution rate in water: 25.0 g of the epoxy crosslinking agent is precisely weighed in a beaker, 225 g of water (25° C.) is added thereto, and the resultant is vigorously stirred and mixed at room temperature (23° C.±2° C.) for 15 minutes, after which the resulting mixture is left to stand for 1 hour, and the volume (mL) of an oily matter precipitated on the bottom of the beaker is subsequently measured to calculate the dissolution rate in water using the following equation:
Dissolution rate in water (%)=(25.0−(Volume of oily matter (mL)×Density of epoxy crosslinking agent (g/mL))/25.0×100.

### Claim 2

A dip molding emulsion comprising, at least:
an elastomer that contains a (meth)acrylonitrile-derived structural unit, an unsaturated carboxylic acid-derived structural unit, and a butadiene-derived structural unit in a polymer main chain;
an epoxy crosslinking agent;
water; and
a pH modifier,
wherein
the elastomer contains the (meth)acrylonitrile-derived structural unit in an amount of 20% by weight to 40% by weight, the unsaturated carboxylic acid-derived structural unit in an amount of 1% by weight to 10% by weight, and the butadiene-derived structural unit in an amount of 50% by weight to 75% by weight, and
the epoxy crosslinking agent consists of an epoxy compound having a basic skeleton that contains plural glycidyl ether groups and alicyclic, aliphatic, or aromatic hydrocarbons in one molecule,
the epoxy crosslinking agent has an average number of epoxy groups per molecule of greater than 2.0, and
the epoxy crosslinking agent has an MIBK/water distribution ratio of 27% or higher as determined by the following measurement method:
Method of measuring the MIBK/water distribution ratio: in a test tube, 5.0 g of water, 5.0 g of methyl isobutyl ketone (MIBK) and 0.5 g of the epoxy crosslinking agent are precisely weighed and mixed with stirring at 23° C.±2° C. for 3 minutes, and the resulting mixture is centrifuged at 1.0×103 G for 10 minutes and thereby separated into an aqueous layer and an MIBK layer, after which the MIBK layer is fractionated and weighed to calculate the MIBK/water distribution ratio using the following equation:
MIBK/water distribution ratio (%)=(Weight of separated MIBK layer (g)−Weight of MIBK before separation (g))/Weight of added crosslinking agent (g)×100
this measurement is performed three times, and an average value thereof is defined as the MIBK/water distribution ratio.

### Claim 3 (depends on 2)

The dip molding emulsion according to claim 2, wherein the epoxy crosslinking agent has an MIBK/water distribution ratio of 50% or higher.

### Claim 4 (depends on 2)

The dip molding emulsion according to claim 2, further comprising a dispersant of the epoxy crosslinking agent.

### Claim 5 (depends on 4)

The dip molding emulsion according to claim 4, wherein the dispersant of the epoxy crosslinking agent is at least one selected from the group consisting of monohydric lower alcohols, glycols represented by the following Formula (1), ethers represented by the following Formula (2), and esters represented by the following Formula (3):
HO—(CH2CHR1—O)n1—H (1)
[in Formula (1), R1 represents hydrogen or a methyl group; and n1 represents an integer of 1 to 3]
R2O—(CH2CHR1—O)n2—R3 (2)
[in Formula (2), R1 represents hydrogen or a methyl group; R2 represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms; R3 represents hydrogen or an aliphatic hydrocarbon group having 1 to 3 carbon atoms; and n2 represents an integer of 0 to 3]
R2O—(CH2CHR1—O)n3—(C═O)—CH3 (3)
[in Formula (3), R1 represents hydrogen or a methyl group; R2 represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms; and n3 represents an integer of 0 to 3].

### Claim 6 (depends on 2)

The dip molding emulsion according to claim 2, wherein the epoxy crosslinking agent is added to the dip molding emulsion in an amount of 0.1 parts by weight to 5.0 parts by weight with respect to 100 parts by weight of the elastomer contained in the dip molding emulsion.

### Claim 7 (depends on 2)

The dip molding emulsion according to claim 2, further comprising zinc oxide and/or an aluminum complex as a metal crosslinking agent(s).

### Claim 8 (depends on 7)

The dip molding emulsion according to claim 7, wherein the metal crosslinking agent is added to the dip molding emulsion in an amount of 0.2 parts by weight to 4.0 parts by weight with respect to 100 parts by weight of the elastomer.

### Claim 9 (depends on 2)

The dip molding emulsion according to claim 2, having a pot life of 3 days or longer.

### Claim 10 (depends on 2)

A method of producing a glove, the method comprising:
(1) a step of immersing a glove forming mold in a liquid coagulant containing calcium ions so as to allow the coagulant to adhere to the glove forming mold;
(2) a step of stirring the dip molding emulsion according to claim 2 whose pH has been adjusted to 9.0 or higher with the pH modifier (maturation step);
(3) a dipping step of immersing the glove forming mold, to which the coagulant has adhered in the step (1), in the dip molding emulsion subjected to the step (2) so as to coagulate the dip molding emulsion on the glove forming mold and thereby form a film;
(4) a gelling step of gelling the film thus formed on the glove forming mold to prepare a cured film precursor, in which gelling step the glove forming mold is left to stand at a temperature of 21° C. to 140° C. for 20 seconds or longer;
(5) a leaching step of removing impurities from the cured film precursor thus formed on the glove forming mold;
(6) a beading step of, after the leaching step, making a roll in a cuff portion of the resulting glove; and
(7) a curing step of heating and drying the cured film precursor eventually at 70° C. to 150° C. for 10 minutes to 30 minutes to obtain a cured film,
which steps (3) to (7) are performed in the order mentioned.

### Claim 11 (depends on 10)

The method of producing a glove according to claim 10, wherein the steps (2) and (3) are performed over a total of 72 hours or longer.

### Claim 12 (depends on 10)

The method of producing a glove according to claim 10, wherein the steps (3) and (4) are repeated twice in the order mentioned.

### Claim 13 (depends on 10)

The method of producing a glove according to claim 10, further comprising, between the steps (6) and (7), a precuring step of heating and drying the cured film precursor at a temperature lower than the temperature of the step (7).

### Claim 14 (depends on 10)

A glove produced by the method according to claim 10.

### Claim 15 (depends on 14)

The glove according to claim 14, wherein the cured film has a fatigue durability of 240 minutes or longer and a tensile strength of 20 MPa or higher as determined by the following respective test methods:
Fatigue durability test method: after preparing a #1 dumbbell test piece of 120 mm in length according to JIS K6251 from the cured film, the thus obtained test piece is repeatedly stretched in the lengthwise direction between a maximum length of 195 mm and a minimum length of 147 mm over a period of 12.8 seconds by pulling an upper part of the test piece with a lower part of the test piece being immobilized and immersed in an artificial sweat solution up to a length of 60 mm, and the time until the test piece is torn is measured; and
Tensile strength test method: a #5 dumbbell test piece according to JIS K6251 is cut out from the cured film, and the tensile strength (MPa) thereof is measured using a TENSILON universal tensile tester RTC-1310A manufactured by A&D Co., Ltd. at a test rate of 500 mm/min, a chuck distance of 75 mm, and a gauge mark distance of 25 mm.

### Claim 16 (depends on 15)

The glove according to claim 15, having a thickness of 0.04 mm to 0.2 mm.