# US 2023/0067566 A1 · Multilayer extreme ultraviolet reflector materials

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0067566 A1
- Document ID: US20230067566A1
- Status: Published application
- Kind: A1
- Application number: 17/461,250
- Filed: 2021-08-30
- Published: 2023-03-02
- Earliest claimed: 2021-08-30
- Assignees: Applied Materials, Inc.
- Applicants: Applied Materials, Inc.
- Inventors: Wen Xiao; Binni Varghese; Vibhu Jindal
- Web page: https://patentgrep.com/patent/US20230067566A1

## CPC

- G03F 1/24: Reflection masks; Preparation thereof
- G03F 1/52: Reflectors
- G03F: PHOTOMECHANICAL PRODUCTION OF TEXTURED OR PATTERNED SURFACES, e.g. FOR PRINTING, FOR PROCESSING OF SEMICONDUCTOR DEVICES; MATERIALS THEREFOR; ORIGINALS THEREFOR; APPARATUS SPECIALLY ADAPTED THEREFOR; (phototypographic composing devices B41B; photosensitive materials or processes for photographic purposes G03C; electrophotography, sensitive layers or processes therefor G03G)

## Abstract

Extreme ultraviolet (EUV) mask blanks, production systems therefor, and methods of increasing multilayer film reflectance are disclosed. The EUV mask blanks comprise a bilayer film on a substrate. The bilayer film comprises a first film layer including silicon (Si), and a second film layer comprising an element selected from the group consisting of ruthenium (Ru), nickel (Ni), cobalt (Co), tungsten (W), iron (Fe), titanium (Ti) and silicides thereof. Some EUV mask blanks further comprise a multilayer reflective stack comprising alternating layers on the bilayer film and a capping layer on the multilayer reflective stack. Some EUV mask blanks include a smoothing layer selected from the group consisting of molybdenum silicide (MoSi), boron carbide (B4C) and silicon nitride (SiN) on the multilayer reflective stack, a capping layer on the smoothing layer, and an absorber layer on the capping layer.

## Claims

### Claim 1

An extreme ultraviolet (EUV) mask blank comprising:
a bilayer film on a substrate, the bilayer film comprising a first film layer including silicon (Si), and a second film layer comprising an element selected from the group consisting of ruthenium (Ru), nickel (Ni), cobalt (Co), tungsten (W), iron (Fe), titanium (Ti) and silicides thereof;
a multilayer reflective stack on the bilayer film, the multilayer reflective stack comprising alternating layers; and
a capping layer on the multilayer reflective stack.

### Claim 2 (depends on 1)

The EUV mask blank of claim 1, further comprising a smoothing layer on the multilayer reflective stack and the capping layer on the smoothing layer, the smoothing layer selected from the group consisting of molybdenum silicide (MoSi), boron carbide (B4C) and silicon nitride (SiN).

### Claim 3 (depends on 2)

The EUV mask blank of claim 2, wherein the first film layer has a thickness in a range of 3 nm to 5 nm and the second film layer has a thickness in a range of 1 nm to 3 nm.

### Claim 4 (depends on 3)

The EUV mask blank of claim 3, wherein the second film layer comprises a trilayer comprising a first layer comprising a silicide of one or more of ruthenium (Ru), nickel (Ni), cobalt (Co), tungsten (W), iron (Fe), and titanium (Ti), a second layer including an element selected from the group consisting of ruthenium (Ru), nickel (Ni), cobalt (Co), tungsten (W), iron (Fe), and titanium (Ti), and a third layer comprising a silicide of one or more of ruthenium (Ru), nickel (Ni), cobalt (Co), tungsten (W), iron (Fe), and titanium (Ti) after annealing the EUV mask blank.

### Claim 5 (depends on 4)

The EUV mask blank of claim 4, wherein each of the first layer and the third layer has a thickness in a range of 1 nm to 3 nm.

### Claim 6 (depends on 1)

The EUV mask blank of claim 1, further comprising at least one interface layer between each of the alternating layers of the multilayer reflective stack.

### Claim 7 (depends on 6)

The EUV mask blank of claim 6, wherein each of the at least one interface layer has a thickness that does not increase more than 20% after annealing.

### Claim 8 (depends on 7)

The EUV mask blank of claim 7, wherein the at least one interface layer has a thickness in a range of from 0.5 nm to 2 nm.

### Claim 9 (depends on 2)

The EUV mask blank of claim 2, wherein the smoothing layer has a thickness in a range of 0.5 nm to 2 nm.

### Claim 10 (depends on 9)

The EUV mask blank of claim 9, wherein the EUV mask blank has a surface roughness in a range of from 0.10 nm to 0.20 nm.

### Claim 11 (depends on 1)

The EUV mask blank of claim 1, wherein the capping layer has a thickness in a range of from 2 nm to 5 nm.

### Claim 12 (depends on 11)

The EUV mask blank of claim 11, wherein the capping layer comprises ruthenium (Ru).

### Claim 13

A method of increasing reflectance of a multilayer film, the method comprising:
forming a bilayer film on a substrate comprising a first film layer and a second film layer, the first film layer including silicon (Si), and the second film layer comprising an element selected from the group consisting of ruthenium (Ru), nickel (Ni), cobalt (Co), tungsten (W), iron (Fe), titanium (Ti), and silicides thereof;
forming a multilayer reflective stack comprising alternating layers on the bilayer film;
forming a capping layer on the multilayer reflective stack; and
annealing the multilayer film.

### Claim 14 (depends on 13)

The method of claim 13, further comprising forming a smoothing layer on the multilayer reflective stack and forming the capping layer on the smoothing layer, the smoothing layer selected from the group consisting of molybdenum silicide (MoSi), boron carbide (B4C) and silicon nitride (SiN).

### Claim 15 (depends on 14)

The method of claim 14, wherein the multilayer film has a reflectance of about 66.8% before annealing.

### Claim 16 (depends on 14)

The method of claim 14, wherein the multilayer film has a reflectance of about 66.1 % after annealing.

### Claim 17 (depends on 14)

The method of claim 14, wherein forming the smoothing layer reduces a surface roughness of the multilayer film compared to a multilayer film not having a smoothing layer.

### Claim 18 (depends on 17)

The method of claim 17, wherein the surface roughness of the multilayer film is in a range of from a range of 0.10 nm to 0.20 nm.

### Claim 19 (depends on 14)

The method of claim 14, wherein a stress in the multilayer film is reduced from about 600 nm before annealing to about 200 nm after annealing.

### Claim 20 (depends on 13)

The method of claim 13, wherein annealing the multilayer film is performed at a temperature in a range of from 180° C. to 250° C. for a time period in a range of from 5 minutes to 60 minutes.