# US 2023/0066827 A1 · Method of manufacturing negative electrode

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0066827 A1
- Document ID: US20230066827A1
- Status: Published application
- Kind: A1
- Application number: 17/796,838
- Filed: 2021-03-23
- Published: 2023-03-02
- Earliest claimed: 2020-03-27
- Assignees: LG Energy Solution, Ltd.
- Applicants: LG Energy Solution, Ltd.
- Inventors: Oh Byong CHAE; Ye Ri KIM; Su Yeon LEE; Seo Young JEON; Seung Hae HWANG
- Web page: https://patentgrep.com/patent/US20230066827A1

## CPC

- H01M 4/134: Electrodes based on metals, Si or alloys
- H01M 4/0438: {by electrochemical processing (electroless electrochemical plating C23C18/54)}
- H01M 4/0445: {Forming after manufacture of the electrode, e.g. first charge, cycling}
- H01M 4/0452: {from solutions}
- H01M 4/0459: {Electrochemical doping, intercalation, occlusion or alloying}
- H01M 4/0495: {Chemical alloying}
- H01M 4/13: Electrodes for accumulators with non-aqueous electrolyte, e.g. for lithium-accumulators; Processes of manufacture thereof
- H01M 4/133: Electrodes based on carbonaceous material, e.g. graphite-intercalation compounds or CFx
- H01M 4/139: Processes of manufacture
- H01M 4/1393: of electrodes based on carbonaceous material, e.g. graphite-intercalation compounds or CFx
- H01M 4/364: {as mixtures}
- H01M 4/483: {for non-aqueous cells (H01M4/485 takes precedence)}
- H01M 4/587: for inserting or intercalating light metals
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- H01M 10/0587: of accumulators having only wound construction elements, i.e. wound positive electrodes, wound negative electrodes and wound separators
- H01M 4/0461: {Electrochemical alloying}
- H01M 2004/027: {Negative electrodes}
- Y02E 60/10: Energy storage using batteries
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

A method of manufacturing a negative electrode includes providing a negative electrode roll on which a negative electrode structure including a negative electrode current collector, a first negative electrode active material layer formed on one side of the negative electrode current collector, and a second negative electrode active material layer formed on the other side of the negative electrode current collector is wound, preparing a pre-lithiation bath including an impregnation section and a pre-lithiation section and containing a pre-lithiation solution, unwinding the negative electrode structure, moving the negative electrode structure to the impregnation section, and impregnating the negative electrode structure with the pre-lithiation solution; and pre-lithiating the negative electrode structure by moving the same from the impregnation section to the pre-lithiation section. The pre-lithiation is carried out by alternately electrochemically charging the first negative electrode active material layer and the second negative electrode active material layer in the pre-lithiation section.

## Claims

### Claim 1

A method of manufacturing a negative electrode, comprising:
providing a negative electrode roll on which a negative electrode structure including a negative electrode current collector, a first negative electrode active material layer formed on one side of the negative electrode current collector, and a second negative electrode active material layer formed on the other side of the negative electrode current collector is wound;
preparing a pre-lithiation bath including an impregnation section and a pre-lithiation section and containing a pre-lithiation solution, wherein the impregnation section and the pre-lithiation section are partitioned and sequentially provided;
unwinding the negative electrode structure from the negative electrode roll, and moving the negative electrode structure to the impregnation section and impregnating the negative electrode structure with the pre-lithiation solution to provide an impregnated negative electrode structure; and
pre-lithiating the impregnated negative electrode structure by moving the impregnated negative electrode structure from the impregnation section to the pre-lithiation section to provide a pre-lithiated negative electrode structure,
wherein the pre-lithiating of the impregnated negative electrode structure is carried out by alternately electrochemically charging the first negative electrode active material layer and the second negative electrode active material layer in the pre-lithiation section.

### Claim 2 (depends on 1)

The method of claim 1, wherein the pre-lithiating of the negative electrode structure is carried out by:
disposing a first lithium metal counter electrode facing and spaced apart from the first negative electrode active material layer and a second lithium metal counter electrode facing and spaced apart from the second negative electrode active material layer in the pre-lithiation section;
connecting the first negative electrode active material layer and the first lithium metal counter electrode through a first electrochemical charger/discharger and connecting the second negative electrode active material layer and the second lithium metal counter electrode through a second electrochemical charger/discharger; and
alternately operating the first electrochemical charger/discharger and the second electrochemical charger/discharger to alternately electrochemically charge the first negative electrode active material layer and the second negative electrode active material layer.

### Claim 3 (depends on 1)

The method of claim 1, wherein the pre-lithiating of the negative electrode structure is carried out by alternately electrochemically charging the first negative electrode active material layer and the second negative electrode active material layer in two or more cycles in the pre-lithiation section, wherein, in each cycle, the first negative electrode active material layer and the second negative electrode active material layer is electrochemically charged once.

### Claim 4 (depends on 1)

The method of claim 1, wherein the first negative electrode active material layer and the second negative electrode active material layer are alternately electrochemically charged for a period of 0.1 seconds to 80 seconds.

### Claim 5 (depends on 1)

The method of claim 1, wherein the electrochemically charging is carried out using a current of 0.2 mA/cm2 to 10 mA/cm2.

### Claim 6 (depends on 1)

The method of claim 1, wherein the negative electrode structure moves through the pre-lithiation section in 5 minutes to 120 minutes.

### Claim 7 (depends on 1)

The method of claim 1, wherein a time taken for the negative electrode structure to move through the impregnation section is 1 to 10 times a time taken for the impregnated negative electrode structure to move through the pre-lithiation section.

### Claim 8 (depends on 1)

The method of claim 1, wherein the pre-lithiation bath further includes an aging section which is partitioned and sequentially provided after the pre-lithiation section, and
wherein the method further includes aging the pre-lithiated negative electrode structure by moving the pre-lithiated negative electrode structure from the pre-lithiation section to the aging section.

### Claim 9 (depends on 8)

The method of claim 8, wherein a time taken for the pre-lithiated negative electrode structure to move through the aging section is 0.5 to 21 times a time taken for the impregnated negative electrode structure to move through the pre-lithiation section.

### Claim 10 (depends on 1)

The method of claim 1, further comprising:
moving the pre-lithiated negative electrode structure out of the pre-lithiation bath; and
moving the pre-lithiated negative electrode structure to a washing bath containing an organic solvent and
washing the pre-lithiated negative electrode structure to provide a washed negative electrode structure.

### Claim 11 (depends on 10)

The method of claim 10, wherein a time taken for the pre-lithiated negative electrode structure to move through the washing bath is 0.1 to 5 times a time taken for the impregnated negative electrode structure to move through the pre-lithiation section.

### Claim 12 (depends on 10)

The method of claim 10, further comprising drying the washed negative electrode structure.

### Claim 13 (depends on 1)

The method of claim 1, wherein a temperature inside the pre-lithiation bath is in a range of 10° C. to 80° C.

### Claim 14 (depends on 1)

The method of claim 1, wherein each of the first negative electrode active material layer and the second negative electrode active material layer includes a negative electrode active material, and
wherein the negative electrode active material includes one or more selected from among a carbon-based active material and a silicon-based active material.

### Claim 15 (depends on 1)

The method of claim 1, wherein, in the pre-lithiating of the impregnated negative electrode structure, the first negative electrode active material layer and the second negative electrode active material layer are each independently electrochemically charged to a state-of-charge (SoC) of 5% to 50%.