# US 2023/0058767 A1 · Method for manufacturing precious metal alloys and precious metal alloys thus obtained

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0058767 A1
- Document ID: US20230058767A1
- Status: Published application
- Kind: A1
- Application number: 17/977,198
- Filed: 2022-10-31
- Published: 2023-02-23
- Earliest claimed: 2018-12-07
- Assignees: The Swatch Group Research and Development Ltd
- Applicants: The Swatch Group Research and Development Ltd
- Inventors: Csilla MIKO; Rémi GROSJEAN; Jean-Luc BAZIN; David PORTEHAULT; Yann LE GODEC; Simon DELACROIX; Fernando IGOA SALDANA
- Web page: https://patentgrep.com/patent/US20230058767A1

## CPC

- B22F 3/15: Hot isostatic pressing
- B22F 1/07: Metallic powder characterised by particles having a nanoscale microstructure (nanosized particles B22F1/054)
- B22F 3/1007: {Atmosphere (B22F3/1021 takes precedence)}
- B22F 3/105: by using electric current {other than for infrared radiant energy}, laser radiation or plasma (B22F3/11 takes precedence){; by ultrasonic bonding (B22F3/115 takes precedence)}
- B22F 9/04: starting from solid material, e.g. by crushing, grinding or milling ({C22C1/1084 takes precedence}; crushing, grinding or milling, in general, see the relevant subclasses, e.g. B02C)
- B22F 10/12: by photopolymerisation, e.g. stereolithography [SLA] or digital light processing [DLP]
- B22F 10/14: by jetting of binder onto a bed of metal powder
- B22F 10/16: by embedding the binder within the powder bed
- B22F 10/18: by mixing binder with metal in filament form, e.g. fused filament fabrication [FFF]
- B22F 10/20: Direct sintering or melting
- B22F 10/28: Powder bed fusion, e.g. selective laser melting [SLM] or electron beam melting [EBM]
- B22F 10/34: of powder characteristics, e.g. density, oxidation or flowability
- B33Y 70/00: Materials specially adapted for additive manufacturing
- C22C 1/05: Mixtures of metal powder with non-metallic powder (C22C1/08 takes precedence)
- C22C 1/051: Making hard metals based on borides, carbides, nitrides, oxides or silicides; Preparation of the powder mixture used as the starting material therefor
- C22C 5/00: Alloys based on noble metals
- C22C 5/02: Alloys based on gold
- C22C 5/04: Alloys based on a platinum group metal
- C22C 5/06: Alloys based on silver
- B22F 2003/1051: {by electric discharge}
- B22F 2998/10: Processes characterised by the sequence of their steps
- B33Y 10/00: Processes of additive manufacturing
- B82Y 40/00: Manufacture or treatment of nanostructures
- Y02P 10/25: Process efficiency
- B22F: WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER (making alloys by powder metallurgy C22C); APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B33Y: ADDITIVE MANUFACTURING, i.e. MANUFACTURING OF THREE-DIMENSIONAL [3D] OBJECTS BY ADDITIVE DEPOSITION, ADDITIVE AGGLOMERATION OR ADDITIVE LAYERING, e.g. BY 3D PRINTING, STEREOLITHOGRAPHY OR SELECTIVE LASER SINTERING
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- B82Y: SPECIFIC USES OR APPLICATIONS OF NANOSTRUCTURES; MEASUREMENT OR ANALYSIS OF NANOSTRUCTURES; MANUFACTURE OR TREATMENT OF NANOSTRUCTURES
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

A method for manufacturing a part by alloying a precious metal with boron, wherein: a quantity of precious metal reduced to powder form is provided; a quantity of a nano-structured micrometric boron powder is provided; the precious metal powder is mixed with the nano-structured micrometric boron powder to obtain a mixture; the mixture is compacted by applying a uniaxial pressure; the mixture is subjected to a spark plasma sintering or flash sintering treatment, or to a hot isostatic pressing (HIP) treatment, to obtain an ingot of a precious metal/boron alloy, and the ingot is machined to obtain the part, or the ingot is reduced to powder form by a micronisation treatment and the powder is treated to obtain the part. Additionally, a gold/boron alloy.

## Claims

### Claim 1

A method for manufacturing a part by alloying a precious metal with boron, the precious metal being selected from the group consisting of gold, silver, platinum, palladium, ruthenium, rhodium and iridium, the method comprising:
providing a quantity of the precious metal reduced to powder form;
providing a quantity of a powder formed by aggregates of micrometric sized particles, and wherein the aggregates are composed of nanometric sized particles comprising boron that is responsible for a reactivity of the powder;
mixing the precious metal reduced to powder form with the powder, to obtain a mixture;
compacting the mixture by applying a uniaxial pressure;
subjecting the mixture to a spark plasma sintering or flash sintering treatment at a pressure in a range of from 0.5 GPa to 10 GPa and at a temperature in a range of from 400° C. to 2,100° C., or to a hot isostatic pressing (HIP) treatment at a pressure in a range of from 80 bar to 2,200 bar and at a temperature in a range of from 400° C. to 2,100° C., to obtain an ingot of an alloy comprising precious metal and boron, and
machining the ingot to obtain the part, or
reducing the ingot to a powder by a micronisation treatment and treating the powder to obtain the part.

### Claim 2 (depends on 1)

The method of claim 1, wherein, to obtain the part, the ingot is reduced to the powder by the micronisation treatment and the powder is inserted into a mould and subjected to a uniaxial or isostatic pressure.

### Claim 3 (depends on 1)

The method of claim 1, wherein, to obtain the part, the ingot is reduced to the powder by the micronisation treatment and the powder is subjected to a three-dimensional additive manufacturing treatment.

### Claim 4 (depends on 3)

The method of claim 3, wherein the three-dimensional additive manufacturing treatment is a direct printing treatment.

### Claim 5 (depends on 4)

The method of claim 4, wherein the direct printing treatment is selected from the group consisting of selective laser melting (SLM) and electron beam (E-beam) melting.

### Claim 6 (depends on 3)

The method of claim 3, wherein the three-dimensional additive manufacturing treatment is an indirect printing treatment.

### Claim 7 (depends on 6)

The method of claim 6, wherein the indirect printing treatment is selected from the group consisting of inkjetting, nanoparticle jetting (NPJ) and Digital Light Projecting (DLP).

### Claim 8 (depends on 1)

The method of claim 1, wherein the ingot is reduced to the powder by the micronisation treatment and the method further comprises:
mixing the powder with a binder, to obtain a feedstock;
producing a green body, a shape thereof corresponding to a part profile, by subjecting the feedstock either to an injection or micro-injection, or to an additive manufacturing technique;
obtaining a brown body by subjecting the green body to eliminating of the binder, referred to as debinding, during which the green body is chemically treated then heat treated in a furnace to burn residual binder, the debinding being carried out in gaseous phase in a nitric acid or oxalic acid atmosphere and at a temperature in a range of from 100° C. to 140° C.; and
subjecting the brown body to a sintering treatment in a protected atmosphere and at a temperature in a range of from 700° C. to 1,800° C. to obtain the part.

### Claim 9 (depends on 8)

The method of claim 8, wherein the green body is produced by subjecting the feedstock to the additive manufacturing technique and the additive manufacturing technique is selected from the group consisting of binder jetting, solvent on granulate jetting, FDM or micro-extrusion.

### Claim 10 (depends on 8)

The method of claim 8, wherein after the sintering treatment, the part is subjected to a hot isostatic pressing (HIP) post-treatment at a pressure in a range of from 500 bar to 2,200 bar, and at a temperature in a range of from 600° C. to 2,100° C.

### Claim 11 (depends on 8)

The method of claim 8, wherein the binder is selected from the group consisting of polyethylene glycol (PEG), cellulose acetate butyrate (CAB), nano-cellulose, corn starch, sugar, polylactic acid, polyethylene, polypropylene, synthetic wax, natural wax and stearic acid.

### Claim 12 (depends on 11)

The method of claim 11, wherein the precious metal is gold.

### Claim 13 (depends on 1)

The method of claim 1, wherein the gold is 24-karat yellow gold and is in the form of particles having dimensions of less than 50 μm.

### Claim 14 (depends on 1)

The method of claim 1, wherein the nano-structured micrometric boron powder is selected from the group consisting of NiB, CoB, YB4 and YB6.

### Claim 15 (depends on 14)

The method of claim 14, wherein the nano-structured micrometric boron powder is formed of particles whose dimensions are in a range of from 5 nm to 12 nm and which are formed of a core constituted by HfB2, whose structure is crystalline, and of a layer of amorphous boron, wherein the layer coats the core and has a thickness of several nanometres, and the particles are agglomerated with one another to form three-dimensional structures, the dimensions of which are in a micrometric range.

### Claim 16 (depends on 15)

The method of claim 15, wherein a specific surface area of the nano-structured micrometric boron powder is 700 m2 for 1 g of powder.

### Claim 17 (depends on 1)

The method of claim 1, wherein the nano-structured micrometric powder is formed of particles whose geometrical dimensions are in a range of from 25 to 999 nm and which are made of boron in proportions by weight of greater than 95%, the remainder being constituted by unavoidable impurities originating from synthesis of the nano-structured micrometric powder and which are one or more of the following elements: carbon, nitrogen, oxygen, potassium, sodium, chlorine, iodine, caesium, lithium, rubidium and magnesium, the particles having a geometric value in a nanometric range responsible for a reactivity of the nano-structured micrometric powder.

### Claim 18 (depends on 17)

The method of claim 17, wherein a specific surface area of the nano-structured micrometric boron powder is at least 100 m2 for 1 g of powder.

### Claim 19 (depends on 1)

The method of claim 1, wherein the nano-structured micrometric powder takes the form of particles whose dimensions do not exceed 25 nm and which are made of boron in proportions by weight of greater than or equal to 85%, the remainder being constituted by unavoidable impurities originating from synthesis of the nano-structured micrometric powder and which are one or more of the following elements: lithium, sodium, potassium, rubidium, caesium, iodine, chlorine, bromine and fluorine.

### Claim 20

An AuB6 or Au2B12 gold/boron alloy, the latter component being capable of comprising AuB2 inclusions.

### Claim 21 (depends on 20)

The alloy of claim 20, which is 18-karat gold.

### Claim 22 (depends on 20)

The alloy of claim 20, which comprises other alloyed elements.

### Claim 23 (depends on 20)

The alloy of claim 20, which has a density in a range of from 6.6 to 7 g/cm3.

### Claim 24 (depends on 9)

The method of claim 9, wherein after the sintering treatment, the part is subjected to a hot isostatic pressing (HIP) post-treatment at a pressure in a range of from 500 bar to 2,200 bar, and at a temperature in a range of from 600° C. to 2,100° C.

### Claim 25 (depends on 13)

The method of claim 13, wherein the nano-structured micrometric boron powder is selected from the group consisting of NiB, CoB, YB4 and YB6.

### Claim 26 (depends on 25)

The method of claim 25, wherein the nano-structured micrometric boron powder is formed of particles whose dimensions are in a range of from 5 nm to 12 nm and which are formed of a core constituted by HfB2, whose structure is crystalline, and of a layer of amorphous boron, wherein the layer coats the core and has a thickness of several nanometres, and the particles are agglomerated with one another to form three-dimensional structures, the dimensions of which are in a micrometric range.

### Claim 27 (depends on 21)

(The alloy of claim 21, which has a density in a range of from 6.6 to 7 g/cm3.

### Claim 28 (depends on 22)

The alloy of claim 22, which has a density in a range of from 6.6 to 7 g/cm3.