# US 2023/0019472 A1 · Protective coatings for metals

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2023/0019472 A1
- Document ID: US20230019472A1
- Status: Published application
- Kind: A1
- Application number: 17/782,589
- Filed: 2020-12-04
- Published: 2023-01-19
- Earliest claimed: 2019-12-05
- Assignees: MCT Holdings, LLC
- Applicants: MCT Holdings LTD
- Inventors: Agnieszka Mackiewicz
- Web page: https://patentgrep.com/patent/US20230019472A1

## CPC

- C09D 1/02: alkali metal silicates
- C09D 5/08: Anti-corrosive paints
- C23C 22/48: not containing phosphates, hexavalent chromium compounds, fluorides or complex fluorides, molybdates, tungstates, vanadates or oxalates
- C23C 22/50: Treatment of iron or alloys based thereon
- C23C 22/54: Treatment of refractory metals or alloys based thereon
- C23C 22/73: characterised by the process
- C23C 22/78: Pretreatment of the material to be coated
- C23C 22/83: Chemical after-treatment
- C23G 1/02: with acid solutions
- C23G 1/086: {solutions containing HF}
- C23G 1/106: {refractory metals}
- C25D 11/26: of refractory metals or alloys based thereon
- C25D 11/34: of metals or alloys not provided for in groups C25D11/04 - C25D11/32
- C09D: COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR (cosmetics A61K; processes for applying liquids or other fluent materials to surfaces, in general, B05D; staining wood B27K5/02; glazes or vitreous enamels C03C; natural resins, French polish, drying-oils, driers, turpentine, per se, C09F; polishing compositions other than French polish, ski waxes C09G; adhesives or use of materials as adhesives C09J; materials for sealing or packing joints or covers C09K3/10; materials for stopping leaks C09K3/12; processes for the electrolytic or electrophoretic production of coatings C25D)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- C23G: CLEANING OR DE-GREASING OF METALLIC MATERIAL BY CHEMICAL METHODS OTHER THAN ELECTROLYSIS
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR

## Abstract

The present invention relates to metals or metal alloys comprising a protective silicate glass-like coating, and methods for coating the metals or metal alloys. The methods comprise removal of any existing oxide layer from the metal or metal alloy, formation of a new oxide layer on the metal or metal alloy using chemical passivation or exposure to a gaseous oxidising environment, coating the oxidised metal or metal alloy with an aqueous silicate solution, and curing the coating.

## Claims

### Claim at position 1

-33. (canceled)

### Claim 34

A process for preparing a coated metal or metal alloy product, the process comprising:
providing a metal substrate selected from aluminum, an aluminum alloy, titanium, a titanium alloy, or stainless steel;
removing an existing oxide layer from the metal substrate by pickling, mechanical cleaning, or a combination thereof;
forming a new oxide layer on the surface of the metal substrate by contacting the metal substrate with a passivating solution comprising an acid selected from the group consisting of nitric acid, sulfuric acid, phosphoric acid, citric acid, hydrogen peroxide, sodium dichromate, or any combination thereof, and/or exposing the metal substrate to a gaseous oxidizing environment for a period of time of up to 48 hours;
applying a coating of an aqueous silicate solution to the metal substrate oxide layer; and
curing the applied coating on the oxide layer to provide a silicate coating layer by:
a) heating the coated, passive layer to a temperature of at least 200° C.; or
b) exposing the coated, passive layer to an infrared source.

### Claim 35 (depends on 34)

The process of claim 34, wherein the aqueous silicate solution comprises SiO2, M2O, and optionally B2O3, wherein M is selected from Li, Na, K, and a mixture thereof.

### Claim 36 (depends on 34)

The process of claim 34, wherein the existing oxide layer is removed by abrasive blasting and the new oxide layer is formed by exposing the metal substrate to air for up to about 48 hours.

### Claim 37 (depends on 36)

The process of claim 36, wherein the new oxide layer is formed by exposing the metal substrate to air for up to about 24 hours.

### Claim 38 (depends on 36)

The process of claim 36, further comprising a step of washing the metal substrate prior to applying the coating of aqueous silicate solution.

### Claim 39 (depends on 34)

The process of claim 34, wherein the existing oxide layer is removed from the metal substrate by pickling using an acidic pickling solution comprising nitric acid, hydrofluoric acid, chloric acid, sulfuric acid, phosphoric acid, sodium persulfate, hydrogen peroxide, or a combination thereof.

### Claim 40 (depends on 39)

The process of claim 39, wherein the pickling solution comprises nitric acid and/or hydrofluoric acid.

### Claim 41 (depends on 39)

The process of claim 39, wherein the acidic pickling solution comprises 10%-20% v/v (150 g/L-300 g/L) of 70% nitric acid and from 1% to 2% v/v (12 g/L-24 g/L) of 60% hydrofluoric acid, optionally wherein the acidic pickling solution comprises 15% v/v (225 g/L) of 70% nitric acid and 1.5% v/v (18 g/L) of 60% hydrofluoric acid.

### Claim 42 (depends on 39)

The process of claim 39, wherein the acidic pickling solution has a nitric acid to hydrofluoric acid percentage ratio of 10:1.

### Claim 43 (depends on 39)

The process of claim 39 wherein the pickling is carried out for at least 1 minute at a temperature of at least 15° C.

### Claim 44 (depends on 34)

The process of claim 34, wherein the passivating solution comprises from about 1% to about 30% citric acid or from about 15% to about 30% v/v of 70% nitric acid.

### Claim 45 (depends on 44)

The process of claim 44, wherein the passivation is conducted for at least 3 minutes at a temperature of between 15° C. and 80° C.

### Claim 46 (depends on 34)

The process of claim 34, wherein the passivating solution comprises from 15% to 30% v/v of 70% nitric acid, and wherein the step of chemical passivation is conducted for at least 20 minutes at a temperature of from 15° C. to 60° C.

### Claim 47 (depends on 34)

The process of claim 34, wherein the passivating solution comprises from 1% to 15% w/v of citric acid, and wherein the step of chemical passivation is conducted for at least 4 minutes at a temperature of from 15° C. to 70° C.

### Claim 48 (depends on 34)

The process of claim 34, wherein passivation is carried out using:
a) 20%-25% v/v of 70% nitric acid solution at room temperature for a minimum of 30 minutes;
b) 20%-25% v/v of 70% nitric acid solution heated to 45° C.-60° C. for a minimum of 20 minutes;
c) 4%-1% w/v citric acid solution at temperature 20° C.-50° C. for a minimum of 20 minutes;
d) 4%-10% w/v citric acid solution at temperature 50° C.-60° C. for a minimum of 10 minutes;
e) 4%-10% w/v citric acid solution at temperature 60° C.-70° C. for a minimum of 4 minutes;
f) 22.5% v/v of 70% nitric acid solution at ambient temperature for about 30 minutes; or
g) 7% w/v of citric acid solution at ambient temperature for about 30 minutes.

### Claim 49 (depends on 34)

The process of claim 34, wherein the step of forming a new oxide layer on the surface of the metal substrate comprises exposing the metal substrate to a gaseous oxidizing environment for about 10 to about 120 minutes at a temperature of from about 15° C. to about 25° C.

### Claim 50 (depends on 34)

The process of claim 34, comprising:
cleaning the surface of the metal substrate;
removing an existing oxide layer from the metal substrate by pickling using an acidic pickling solution comprising nitric acid and hydrofluoric acid having a pH of about 1;
forming an oxide layer on the surface of the metal substrate using a chemical passivating solution comprising nitric acid or citric acid and having a pH of about 1;
applying a coating of an aqueous silicate solution to the metal substrate, wherein the aqueous silicate solution has a pH of from about 10 to about 13, comprises SiO2, M2O, and B2O3, wherein M is selected from Li, Na, K, or a mixture thereof, and has a ratio of SiO2 to M2O of from about 3.8 to about 2.0 and a ratio of SiO2 to B2O3 of from about 10:1 to about 200:1; and
curing the silicate solution on the oxide layer to provide a silicate coating layer by:
heating the coated, passive layer to a temperature of at least 200° C.; or
exposing the coated, passive layer to an infrared source.

### Claim 51 (depends on 34)

The process of claim 34, wherein the method comprises heating the coated, passive layer to a temperature of at least 230° C.

### Claim 52 (depends on 50)

The process of claim 50, wherein the pickling solution comprises 10%-20% v/v (150 g/L-300 g/L) of 70% nitric acid and from 1% to 2% v/v (12 g/L-24 g/L) of 60% hydrofluoric acid.

### Claim 53 (depends on 50)

The process of claim 50, wherein the passivating solution comprises 15% to 30% v/v of 70% nitric acid, and passivation is conducted for at least about 20 minutes and at a temperature of from about 15° C. to about 60° C.

### Claim 54 (depends on 50)

The process of claim 50, wherein the passivating solution comprises 1% to 15% w/v of citric acid, and passivation is conducted for at least about 4 minutes and at a temperature of from about 21° C. to about 70° C.

### Claim 55 (depends on 34)

The process of claim 34, comprising removing the existing oxide layer from the metal substrate by abrasive blasting;
washing the blasted metal substrate;
exposing the metal substrate to air for up to 48 hours at room temperature to form a new oxide layer on the surface of the metal substrate;
applying a coating of an aqueous silicate solution to the new metal substrate oxide layer, wherein the aqueous silicate solution has a pH of from 10 to 13, that comprises SiO2, M2O, and optionally B2O3, wherein M is selected from Li, Na, K, or a mixture thereof, and has a ratio of SiO2 to M2O of from about 3.8 to about 2 and, if B2O3 is present, a ratio of SiO2 to B2O3 of from about 10:1 to about 200:1;
curing the applied coating on the new oxide layer to provide a silicate coating layer by:
heating the coating to a temperature of at least 200° C.; or
exposing the coating to an infrared source.

### Claim 56 (depends on 55)

The process of claim 55, comprising heating the coating to a temperature of at least about 230° C.

### Claim 57 (depends on 34)

The process of claim 34, wherein the cured silicate coating layer has a thickness of less than 5 μm and/or the coated oxide layer prepared by the passivation has a thickness of less than about 50 μm.

### Claim 58 (depends on 34)

The process of claim 34, wherein the method comprises a step of cleaning the surface of the metal substrate prior to removing an existing oxide layer, and the step of cleaning comprises removing any grease from the surface of the metal substrate.

### Claim 59 (depends on 34)

The process of claim 34, wherein the method comprises a step of cleaning the surface of the metal substrate, and the step of cleaning comprises an abrasive treatment of the surface of the metal substrate.