# US 2022/0367798 A1 · Laser-Written Submicron Pixels with Tunable Circular Polarization and Write-Read-Erase-Reuse Capability on a Nano Material or Two-Dimensional Heterostructure at Room Temperature

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0367798 A1
- Document ID: US20220367798A1
- Status: Published application
- Kind: A1
- Application number: 17/690,263
- Filed: 2022-03-09
- Published: 2022-11-17
- Earliest claimed: 2021-05-12
- Assignees: The Government of the United States of America, as represented by the Secretary of the Navy
- Applicants: The Government of the United States of America, as represented by the Secretary of the Navy
- Inventors: Zachariah B. Hennighausen; Kathleen M. McCreary; Olaf M.J. van 't Erve; Berend T. Jonker
- Web page: https://patentgrep.com/patent/US20220367798A1

## CPC

- G11B 7/243: comprising inorganic materials only, e.g. ablative layers
- H10N 70/257: {having switching assisted by radiation or particle beam, e.g. optically controlled devices}
- B82Y 10/00: Nanotechnology for information processing, storage or transmission, e.g. quantum computing or single electron logic
- B82Y 20/00: Nanooptics, e.g. quantum optics or photonic crystals
- B82Y 40/00: Manufacture or treatment of nanostructures
- G11B 7/2433: Metals or elements of Groups 13, 14, 15 or 16 of the Periodic Table, e.g. B, Si, Ge, As, Sb, Bi, Se or Te
- G11C 7/005: {with combined beam-and individual cell access}
- H10N 70/023: {by chemical vapor deposition, e.g. MOCVD, ALD}
- H10N 70/8613: {Heating or cooling means other than resistive heating electrodes, e.g. heater in parallel}
- H10N 70/8825: {Selenides, e.g. GeSe}
- H10N 70/883: {Oxides or nitrides}
- B82Y 30/00: Nanotechnology for materials or surface science, e.g. nanocomposites
- G11B 2007/24324: {Sulfur}
- G11B: INFORMATION STORAGE BASED ON RELATIVE MOVEMENT BETWEEN RECORD CARRIER AND TRANSDUCER (recording measured values in a way that does not require playback through a transducer G01D9/00; recording or playback apparatus using mechanically marked tape, e.g. punched paper tape, or using unit records, e.g. punched or magnetically marked cards G06K; transferring data from one type of record carrier to another G06K1/18; circuits for coupling output of reproducer to radio receiver H04B1/20; gramophone pick-ups or like acoustic electromechanical transducers or circuits therefor H04R)
- H10N: ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- B82Y: SPECIFIC USES OR APPLICATIONS OF NANOSTRUCTURES; MEASUREMENT OR ANALYSIS OF NANOSTRUCTURES; MANUFACTURE OR TREATMENT OF NANOSTRUCTURES
- G11C: STATIC STORES (semiconductor memory devices H10B)

## Abstract

A method of laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on Bi2Se3/WS2 at room temperature, comprising the steps of applying a laser to the Bi2Se3/WS2, writing a submicron pixel, wherein the submicron pixel has a circular polarization, modifying the circular polarization, allowing the circular polarization to be tuned across a range of 39.9%, tuning photoluminescence intensity, and tuning photoluminescence peak position. A method of growing Bi2Se3/WS2 as a nano-material or two-dimensional heterostructure for laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on the Bi2Se3/WS2 heterostructure at room temperature.

## Claims

### Claim 1

A method of laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on a nano-material or two-dimensional heterostructure at room temperature, comprising the steps of:
applying a laser to a nano-material or two-dimensional heterostructure;
writing a submicron pixel;
wherein the submicron pixel has a circular polarization;
modifying the circular polarization;
allowing the circular polarization to be tuned across a range of 39.9%;
tuning photoluminescence intensity across a factor of 161 times; and
tuning photoluminescence peak position across a range of 38 meV.

### Claim 2 (depends on 1)

The method of laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on a nano-material or two-dimensional heterostructure at room temperature of claim 1
wherein the nano-material or two-dimensional heterostructure comprises Bi2Se2.

### Claim 3 (depends on 2)

The method of laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on a nano-material or two-dimensional heterostructure at room temperature of claim 2, comprising the additional steps of:
applying the laser in an atmosphere absent of oxygen;
tuning the circular polarization;
tuning the photoluminescence intensity;
tuning the photoluminescence peak position; and
enabling the material to be controllably erased and changes reversed.

### Claim 4 (depends on 3)

The method of laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on a nano-material or two-dimensional heterostructure at room temperature of claim 3
wherein the nano-material or two-dimensional heterostructure comprises Bi2Se3/WS2 and
wherein the nano-material or two-dimensional heterostructure is reusable.

### Claim 5 (depends on 4)

The method of laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on a nano-material or two-dimensional heterostructure at room temperature of claim 4
wherein the steps occur at room temperature.

### Claim 6 (depends on 5)

The method of laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on a nano-material or two-dimensional heterostructure at room temperature of claim 5
wherein the laser is a low-power laser.

### Claim 7 (depends on 6)

The method of laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on a nano-material or two-dimensional heterostructure at room temperature of claim 6
wherein the laser comprises 0.60 micro Watts;
wherein the laser written submicron pixels are written at 814 nm resolution;
wherein the tuning is stable for greater than 106 days; and
wherein the thickness of the SiO2 is 275 nm.

### Claim 8 (depends on 7)

The method of laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on a nano-material or two-dimensional heterostructure at room temperature of claim 7
wherein increasing the laser power increases speed at which the changes are induced.

### Claim 9 (depends on 2)

The method of laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on a nano-material or two-dimensional heterostructure at room temperature of claim 2, further comprising the step of:
providing an oxygen environment;
wherein the pixels are written with submicron resolution using a laser in the oxygen environment.

### Claim 10 (depends on 9)

The method of laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on a nano-material or two-dimensional heterostructure at room temperature of claim 9,
wherein the pixels are written at 814 nm resolution;
wherein the tuning is stable for greater than 334 days; and
wherein the thickness of the SiO2 is 275 nm.

### Claim 11

A method of growing a nano-material or two-dimensional heterostructure for laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on the nano-material or two-dimensional heterostructure at room temperature, comprising the steps of:
providing SiO2/Si substrates;
cleaning the SiO2/Si substrates in acetone, IPA, and Piranha etch;
rinsing the SiO2/Si substrates in deionized water;
positioning at the center of a furnace a first quartz boat containing about 1 g of WO3 powder;
positioning a first SiO2/Si substrate face-down, directly above the WO3 powder;
positioning a second quartz boat containing sulfur powder upstream, outside the furnace-heating zone, for the synthesis of WS2;
positioning a second SiO2/Si substrate above the second quartz boat;
wherein the second SiO2/Si substrate contains perylene-3,4,9,10-tetracarboxylic acid tetrapotassium salt (PTAS) seeding molecules;
wherein the first SiO2/Si substrate is untreated;
allowing the PTAS seeding molecules to be carried downstream to the first substrate which is untreated;
promoting lateral growth of a monolayer WS2;
utilizing pure argon at 65 sccm as the furnace heats to a target temperature;
heating the furnace to a temperature of 825° C.;
adding 10 sccm H2 to the Ar flow and maintaining;
cooling to room temperature; and
resulting in a monolayer WS2.

### Claim 12 (depends on 11)

The method of growing a nano-material or two-dimensional heterostructure for laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on the nano-material or two-dimensional heterostructure at room temperature of claim 11, further comprising the steps of:
growing a layer of Bi2Se3 on top of the monolayer of WS2 using chemical vapor deposition (CVD) in a two-zone furnace with a 2″ quartz tube;
wherein the step of growing a layer of Bi2Se3 on top of the monolayer of WS2 using chemical vapor deposition (CVD) in a two-zone furnace with a 2″ quartz tube comprises the steps of
grinding High-purity Bi2Se3 flakes into a fine dust;
placing in a ceramic boat the fine dust of Bi2Se3;
inserting the ceramic boat into the quartz tube;
pushing the ceramic boat into the center of the first zone of the furnace;
placing the monolayer WS2, which is on an SiO2 substrate, downstream of the Bi2Se3 into the center of the second zone of the furnace;
pumping down the furnace to ˜20 mTorr;
flowing an argon (Ar) carrier gas into the furnace at 80 sccm;
heating the Bi2Se3 to a temperature of 520° C.;
heating the WS2 to a temperature of 210° C.;
heating at a ramp rate of ˜55° C./min; and
growing Bi2Se3/WS2 for 27 min.

### Claim 13 (depends on 12)

The method of growing a nano-material or two-dimensional heterostructure for laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on a nano-material or two-dimensional heterostructure at room temperature of claim 12
wherein 1-3 layers of Bi2Se3 is grown on the monolayer WS2 using CVD; and
wherein the WS2 grows crystalline.

### Claim 14 (depends on 13)

The method of growing a nano-material or two-dimensional heterostructure for laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on a nano-material or two-dimensional heterostructure at room temperature of claim 13
wherein the Bi2Se3/WS2 2D heterostructure comprises complete coverage of Bi2Se3 on the WS2.

### Claim 15 (depends on 14)

The method of growing a nano-material or two-dimensional heterostructure for laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on a nano-material or two-dimensional heterostructure at room temperature of claim 14
wherein monolayer Bi2Se3 flakes several microns in size were grown on the monolayer WS2;
wherein both the Bi2Se3 and the WS2 have long-range crystallinity;
wherein the Bi2Se3 flakes or crystals grow at a 0° twist angle as the most stable configuration; and
wherein the interlayer interaction modulates the growth.

### Claim 16

A method of laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on a nano-material or two-dimensional heterostructure at room temperature, comprising the steps of:
applying a laser to a nano-material or two-dimensional heterostructure;
writing a submicron pixel;
wherein the submicron pixel has a circular polarization;
modifying the circular polarization;
allowing the circular polarization to be tuned across a range of 39.9%;
tuning photoluminescence intensity across a factor of 161 times; and
tuning photoluminescence peak position across a range of 38 meV.
wherein the nano-material or two-dimensional heterostructure comprises Bi2Se3/WS2.

### Claim 17

A nano-material or two-dimensional heterostructure for laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on the nano-material or two-dimensional heterostructure at room temperature, formed by the steps of:
providing SiO2/Si substrates;
cleaning the SiO2/Si substrates in acetone, IPA, and Piranha etch;
rinsing the SiO2/Si substrates in deionized water;
positioning at the center of a furnace a first quartz boat containing about 1 g of WO3 powder;
positioning a first SiO2/Si substrate face-down, directly above the WO3 powder;
positioning a second quartz boat containing sulfur powder upstream, outside the furnace-heating zone, for the synthesis of WS2;
positioning a second SiO2/Si substrate above the second quartz boat;
wherein the second SiO2/Si substrate contains perylene-3,4,9,10-tetracarboxylic acid tetrapotassium salt (PTAS) seeding molecules;
wherein the first SiO2/Si substrate is untreated;
allowing the PTAS seeding molecules to be carried downstream to the first substrate which is untreated;
promoting lateral growth of a monolayer WS2;
utilizing pure argon at 65 sccm as the furnace heats to a target temperature;
heating the furnace to a temperature of 825° C.;
adding 10 sccm H2 to the Ar flow and maintaining;
cooling to room temperature; and
resulting in a monolayer WS2.

### Claim 18 (depends on 17)

The nano-material or two-dimensional heterostructure for laser-writing submicron pixels with tunable circular polarization and write-read-erase-reuse capability on the nano-material or two-dimensional heterostructure at room temperature of claim 17, further comprising the steps of:
growing a layer of Bi2Se3 on top of the monolayer of WS2 using chemical vapor deposition (CVD) in a two-zone furnace with a 2″ quartz tube;
wherein the step of growing a layer of Bi2Se3 on top of the monolayer of WS2 using chemical vapor deposition (CVD) in a two-zone furnace with a 2″ quartz tube comprises the steps of
grinding High-purity Bi2Se3 flakes into a fine dust;
placing in a ceramic boat the fine dust of Bi2Se3;
inserting the ceramic boat into the quartz tube;
pushing the ceramic boat into the center of the first zone of the furnace;
placing the monolayer WS2, which is on an SiO2 substrate, downstream of the Bi2Se3 into the center of the second zone of the furnace;
pumping down the furnace to ˜20 mTorr;
flowing an argon (Ar) carrier gas into the furnace at 80 sccm;
heating the Bi2Se3 to a temperature of 520° C.;
heating the WS2 to a temperature of 210° C.;
heating at a ramp rate of ˜55° C./min; and
growing Bi2Se3/WS2 for 27 min.

### Claim 19

A laser-writing submicron pixel with tunable circular polarization and write-read-erase-reuse capability on a nano-material or two-dimensional heterostructure at room temperature, formed by the steps of:
applying a laser to a nano-material or two-dimensional heterostructure;
wherein the nano-material or two-dimensional heterostructure comprises Bi2Se3/WS2;
wherein the submicron pixel has a circular polarization;
modifying the circular polarization;
allowing the circular polarization to be tuned across a range of 39.9%;
wherein photoluminescence intensity can be tuned across a factor of 161 times; and
wherein photoluminescence peak position can be tuned across a range of 38 meV.