# US 2022/0354095 A1 · Marine ecological engineering construction method, asphalt cement-based coating, and preparation method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0354095 A1
- Document ID: US20220354095A1
- Status: Published application
- Kind: A1
- Application number: 17/830,272
- Filed: 2022-06-01
- Published: 2022-11-10
- Earliest claimed: 2019-12-02
- Assignees: Jianfu LV
- Inventors: Jianfu LV; Fei XU; Mingjun WANG; Zhenzhen CAO
- Web page: https://patentgrep.com/patent/US20220354095A1

## CPC

- A01K 61/77: of monolithic form, e.g. blocks
- A01K 61/54: of bivalves, e.g. oysters or mussels
- C04B 18/027: {Lightweight materials}
- C04B 18/167: Recycled materials, i.e. waste materials reused in the production of the same materials
- C04B 28/02: containing hydraulic cements other than calcium sulfates
- C04B 41/009: {characterised by the material treated}
- C04B 41/478: {Bitumen, asphalt, e.g. paraffin}
- C04B 41/5076: {with masses bonded by inorganic cements (sulfur compositions C04B41/5097)}
- C04B 41/65: with inorganic materials
- C09D 195/00: Coating compositions based on bituminous materials, e.g. asphalt, tar, pitch
- E02B 3/06: Moles; Piers; Quays; Quay walls; Groynes; Breakwaters {; Wave dissipating walls; Quay equipment}
- C04B 2103/0052: {Hydrophobic polymers}
- C04B 2103/54: Pigments; Dyes
- C04B 2111/40: Porous or lightweight materials
- C04B 2111/74: Underwater applications
- Y02A 40/81: Aquaculture, e.g. of fish
- A01K: ANIMAL HUSBANDRY; AVICULTURE; APICULTURE; PISCICULTURE; FISHING; REARING OR BREEDING ANIMALS, NOT OTHERWISE PROVIDED FOR; NEW BREEDS OF ANIMALS
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE
- C09D: COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR (cosmetics A61K; processes for applying liquids or other fluent materials to surfaces, in general, B05D; staining wood B27K5/02; glazes or vitreous enamels C03C; natural resins, French polish, drying-oils, driers, turpentine, per se, C09F; polishing compositions other than French polish, ski waxes C09G; adhesives or use of materials as adhesives C09J; materials for sealing or packing joints or covers C09K3/10; materials for stopping leaks C09K3/12; processes for the electrolytic or electrophoretic production of coatings C25D)
- E02B: HYDRAULIC ENGINEERING (ship-lifting E02C; dredging E02F)
- Y02A: TECHNOLOGIES FOR ADAPTATION TO CLIMATE CHANGE

## Abstract

Disclosed are a marine ecological engineering construction method, an asphalt cement-based coating, and a preparation method thereof. The asphalt cement-based coating can make discarded concrete have the capacity of inducing the settlement of sessile organisms, achieve the purpose of using discarded concrete to construct ecological engineering, and has the characteristics of discarded object recycling and marine ecological restoration.

## Claims

### Claim 1

A construction method for marine ecological engineering by discarded concrete blocks, comprising:
(1) surveying a sea area of a breakwater construction position: surveying dominant species of oysters in the sea area and whether the oysters are attached, surveying air temperature, seawater temperature, dissolved oxygen, plankton, total dissolved inorganic nitrogen, active phosphate, active silicate, Ca2+, Zn2+, K+ and the like for the sea area at different seasons, and surveying typhoon times, strength and the like over the years;
(2) preparing a lightweight concrete settlement substrate with a rough surface for oyster, wherein the shape of the lightweight concrete settlement substrate for oyster is one of the shapes of a slab-shaped settlement substrate, a wave-shaped settlement substrate and a cylindrical settlement substrate;
(3) quantitatively collecting and cultivating oyster larvae: placing the settlement substrate in a larva collection area of local sea area, where the swimming larvae are mainly in metamorphosis period, stopping collecting the larvae once the amount of the settled oyster larvae is 15-25 larvae/100 cm2, and then moving the settlement substrate to a sea area with rich baits for floating cultivation;
(4) treating surfaces of discarded concrete blocks: evaluating the alkalinity, the internal ion concentration and the permeability of the discarded concrete; if the pH is more than 12.5, reducing the alkalinity, and spraying or brushing an emulsified asphalt cement-based coating with high bonding strength and high induction for oyster to settle on the surfaces of the discarded concrete blocks;
(5) placing discarded concrete blocks: in the concentration period of settlement and metamorphosis of oyster planktonic larvae in the local sea area of the next year, adopting a dispersed placement method, placing the discarded concrete blocks with volume of more than 1 m3 individually, and covering each rock with a rope; covering multiple discarded concrete blocks with the volume of less than 1 m3 with the ropes to form a discarded concrete block pile with a volume of 1-5 m3, wherein the internal voidage is 40%-60%; and connecting the rocks by ropes;
(6) placing the oyster settlement substrate in site: conveying the oyster settlement substrate in which the gonad of oysters develops into mature stage in the step (2) to the sea area for constructing the breakwater, placing one lightweight concrete oyster settlement substrate with the rough surface on single discarded concrete block or discarded concrete block pile and fixing the lightweight concrete settlement substrate for oyster on single discarded concrete block or discarded concrete block pile through a rope; in addition, feeding algae or replenishing nutritive salts if necessary according to the planktonic condition of the local sea area; and
(7) monitoring and managing the state of larval settlement: monitoring the settlement condition of oyster larvae on the rock surface; when the larval settlement density is 30 to 40 larvae/100 cm2, moving away the oyster settlement substrate, monitoring the ecological condition of a breakwater for a long time, and providing corresponding measures according to the practical condition.

### Claim 2 (depends on 1)

The construction method for marine ecological engineering by discarded concrete blocks according to claim 1, wherein the settlement substrate for oyster is prepared from the following components in percentage by weight: 21.8-34.5% of a cementitious material, 24.6-37.5% of lightweight coarse aggregate, 15.8-29.6% of lightweight fine aggregate, 8.4-16.4% of water, 0.6-3.0% of a dark pigment, 0.4-2.0% of biological calcium powder, 0.4-2.0% of calcium carbonate powder, 0.2-1.8% of trace elements, 0.15-1.5% of chopped fibers and 0.03-0.18% of a superplasticizer.

### Claim 3 (depends on 2)

The construction method for marine ecological engineering by discarded concrete blocks according to claim 2, wherein in the raw materials of the settlement substrate for oyster, the dark pigment is one or two of iron oxide black, nigrosine, carbon black, antimony sulfide, iron oxide red and organic pigment red; the pigments are modified according to the influence degree on the concrete properties; and one of transparent resin, organosilicon, dimethylsiloxane and a superhydrophobic material is used for modification treatment;
the biological calcium powder is bovine bone powder; the biological calcium carbonate powder comprises one or a combination of more of oyster shell powder, fishbone powder, egg shell powder and coral powder, with fineness of 100-1000 meshes; the 100-500-mesh egg shell powder, coral powder, oyster shell powder and fishbone powder are treated with one or two of acetic acid, silicic acid and sulfurous acid; and the 100-500-mesh bovine bone powder is treated with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid and nitric acid;
the calcium carbonate powder is one or more of calcite powder, chalk powder, limestone powder, marble powder, aragonite powder, travertine powder, processed lightweight calcium carbonate, active calcium carbonate, calcium carbonate whiskers and ultrafine lightweight calcium carbonate, with a fineness of greater than 200 meshes;
the trace elements that are zinc, iron, potassium and phosphorus are selected from natural minerals, industrial products or chemical reagents, including one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, ferric sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and ferric phosphate, and are modified to realize slow release of corresponding ions and to reduce or eliminate adverse effects on the concrete properties; and for eutrophic areas, substances containing nitrogen and phosphorus elements are not selected;
the cementitious material is one of mineral admixture added Portland cement, sulphoaluminate cement and an alkali-activated cementitious material; the mineral admixture in the mineral admixture added Portland cement comprises one or a combination of more of silica fume, slag powder and fly ash; the sulphoaluminate cement comprises one or two of rapid hardening sulphoaluminate cement, high-strength sulphoaluminate cement and expansive sulphoaluminate cement; and the alkali-activated cementitious material comprises one of alkali-activated slag powder, and a combination of alkali-activated slag powder and fly ash;
the lightweight coarse aggregate is one or two of crushed lightweight porous basalt and lightweight ceramsite of which the maximum particle size is less than 20 mm;
the lightweight fine aggregate is one or two of crushed zeolite and lightweight ceramic sand, with a particle size of 0.2 mm to 5 mm;
the chopped fibers are inorganic fibers (12-20 mm in length) and comprise one or more of basalt fibers, alkali-resistant glass fibers and carbon fibers;
wherein preparing the lightweight concrete settlement substrate comprises:
S1, designing different roughness according to the characteristic that oyster larvae prefer to settle on rough substrate surface, and then manufacturing molding form works with different roughness;
S2, weighing a cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water, a dark pigment, biological calcium powder, calcium carbonate powder, trace elements, chopped fibers and a superplasticizer;
S3, firstly putting the lightweight coarse aggregate and the lightweight fine aggregate into a concrete mixer to be mixed for 0.5-1 min; then adding the cementitious material, the dark pigment, the biological calcium powder, the calcium carbonate powder and the trace elements, and continuously mixing for 1-2 min; then adding the chopped fibers, the water and the superplasticizer, and mixing for 2-6 min; then carrying out casting and consolidating after uniformly mixing; and
S4, putting a concrete specimen after demolding into a high-concentration CO2 curing chamber for curing for 0.5-5 h according to the situation so as to reduce the alkalinity of the concrete specimen, and then carrying out standard curing for 28 d or curing according to the actual situation, thus obtaining the concrete settlement substrate with the rough surface for oyster and a good induction effect.

### Claim 4 (depends on 1)

The construction method for marine ecological engineering by discarded concrete blocks according to claim 1, wherein the emulsified asphalt cement-based coating is prepared in ratio by weight: 1 of a cementitious material, 0.4-0.8 of an emulsified asphalt, 0.5-1.3 of sand, 0.10-0.30 of water, 0.02-0.10 of biological calcium powder, 0.02-0.10 of calcium carbonate powder, 0.01-0.08 of trace elements, 0.08-0.15 of acrylic emulsion, and 0.001-0.008 of a superplasticizer.

### Claim 5 (depends on 1)

The construction method for marine ecological engineering by discarded concrete blocks according to claim 1, wherein in the raw materials of the emulsified asphalt cement-based coating, the biological calcium powder is bovine bone powder; the biological calcium carbonate powder comprises one or a combination of more of oyster shell powder, fishbone powder, egg shell powder and coral powder, with fineness of 100-1000 meshes;
wherein the biological calcium powder is modified by a method for treating the 100-500-mesh egg shell powder, coral powder, oyster shell powder and fishbone powder with one or two of acetic acid, silicic acid and sulfurous acid, and treating the 100-500-meshbovine bone powder with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid and nitric acid;
wherein the calcium carbonate powder is calcite powder, chalk powder, limestone powder, marble powder, aragonite powder, travertine powder, and one or more of processed lightweight calcium carbonate, active calcium carbonate, calcium carbonate whiskers and ultrafine lightweight calcium carbonate, with a fineness of greater than 200 meshes;
wherein the trace elements that are zinc, iron, potassium and phosphorus are selected from natural minerals, industrial products or chemical reagents, including one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, ferric sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and ferric phosphate, and are modified to realize slow release of corresponding ions and to reduce or eliminate adverse effects on the concrete properties; and for eutrophic areas, substances containing nitrogen and phosphorus elements are not selected;
wherein the emulsified asphalt is one of cationic emulsified asphalt and anionic emulsified asphalt; the performance indexes of the emulsified asphalt are as follows: the content of evaporation residues is more than 55%, the stability of 5 d is less than or equal to 5%, the sieve diameter is 1.18 mm, and the remaining amount on the sieve is less than or equal to 0.1%;
wherein the cementitious material is one of mineral admixture added Portland cement, sulphoaluminate cement and an alkali-activated cementitious material; the mineral admixture in the mineral admixture added Portland cement comprises one or a combination of more of silica fume, slag powder and fly ash; the sulphoaluminate cement comprises one or two of rapid hardening sulphoaluminate cement, high-strength sulphoaluminate cement and expansive sulphoaluminate cement; and the alkali-activated cementitious material comprises one of alkali-activated slag powder, and a combination of alkali-activated slag powder and fly ash;
wherein the sand is one or more of river sand, machine-made sand or desalinated sea sand, with a particle size of 0.16 mm to 2.36 mm; and
wherein the superplasticizer is one of polycarboxylate superplasticizer and naphthalene-based superplasticizer.

### Claim 6 (depends on 1)

The construction method for marine ecological engineering by discarded concrete blocks according to claim 1, wherein the concentration period of settlement and metamorphosis of oyster planktonic larvae, is April to October.

### Claim 7 (depends on 1)

The construction method for marine ecological engineering by discarded concrete blocks according to claim 1, where in raw materials of the settlement substrate for oyster, comprise, by weight, 0.6-3.0% of a dark pigment, 21.8-34.5% of a cementitious material, 24.6-37.5% of lightweight coarse aggregate, 15.8-29.6% of lightweight fine aggregate, 8.4-16.4% of water, and 0.03-0.18% of a superplasticizer.

### Claim 8 (depends on 1)

The construction method for marine ecological engineering by discarded concrete blocks according to claim 1, wherein the settlement substrate for oyster is specifically prepared from, by weight, 0.4-2.35% of calcium carbonate powder, 21.8-34.5% of a cementitious material, 24.6-37.5% of lightweight coarse aggregate, 15.8-29.6% of lightweight fine aggregate, 8.4-16.4% of water, and 0.03-0.18% of a superplasticizer.

### Claim 9 (depends on 1)

The construction method for marine ecological engineering by discarded concrete blocks according to claim 1, wherein the settlement substrate for oyster is specifically prepared from, by weight, 0.4-2.35% of bovine bone powder, 21.8-34.5% of a cementitious material, 24.6-37.5% of lightweight coarse aggregate, 15.8-29.6% of lightweight fine aggregate, 8.4-16.4% of water, and 0.03-0.18% of a superplasticizer.

### Claim 10 (depends on 1)

The construction method for marine ecological engineering by discarded concrete blocks according to claim 1, wherein the settlement substrate for oyster is specifically prepared from, by weight, 0.6-3.0% of a modified dark pigment, 0.4-2.35% of bovine bone powder, 21.8-34.5% of a cementitious material, 24.6-37.5% of lightweight coarse aggregate, 15.8-29.6% of lightweight fine aggregate, 8.4-16.4% of water, and 0.03-0.18% of a superplasticizer.

### Claim 11

A emulsified asphalt cement-based coating, comprising the following components in ratio by weight: 1 of a cementitious material, 0.4-0.8 of an emulsified asphalt, 0.5-1.3 of sand, 0.10-0.30 of water, 0.02-0.10 of biological calcium powder, 0.02-0.10 of calcium carbonate powder, 0.01-0.08 of trace elements, 0.08-0.15 of acrylic emulsion, and 0.001-0.008 of a superplasticizer.

### Claim 12 (depends on 11)

The emulsified asphalt cement-based coating according to claim 11, wherein the biological calcium powder is bovine bone powder; the biological calcium carbonate powder comprises one or a combination of more of oyster shell powder, fishbone powder, egg shell powder and coral powder, with fineness of 100-1000 meshes.

### Claim 13 (depends on 12)

The emulsified asphalt cement-based coating according to claim 12, wherein the biological calcium powder is modified by a method for treating the 100-500-mesh egg shell powder, coral powder, oyster shell powder and fishbone powder with one or two of acetic acid, silicic acid and sulfurous acid, and treating the 100-500-meshbovine bone powder with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid and nitric acid.

### Claim 14 (depends on 11)

The emulsified asphalt cement-based coating according to claim 11, wherein the calcium carbonate powder is one or more of calcite powder, chalk powder, limestone powder, marble powder, aragonite powder, travertine powder, processed lightweight calcium carbonate, active calcium carbonate, calcium carbonate whiskers and ultrafine lightweight calcium carbonate, with a fineness of greater than 200 meshes.

### Claim 15 (depends on 11)

The emulsified asphalt cement-based coating according to claim 11, wherein the trace elements that are zinc, iron, potassium and phosphorus are selected from natural minerals, industrial products or chemical reagents, including one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, ferric sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and ferric phosphate, and are modified to realize slow release of corresponding ions and to reduce or eliminate adverse effects on the concrete properties; and for eutrophic areas, substances containing nitrogen and phosphorus elements are not selected.

### Claim 16 (depends on 11)

The emulsified asphalt cement-based coating according to claim 11, wherein the emulsified asphalt is one of cationic emulsified asphalt and anionic emulsified asphalt; the performance indexes of the emulsified asphalt are as follows: the content of evaporation residues is more than 55%, the stability of 5 d is less than or equal to 5%, and the remaining amount on the sieve is less than or equal to 0.1%.

### Claim 17 (depends on 11)

The emulsified asphalt cement-based coating according to claim 11, the cementitious material is one of mineral admixture added Portland cement, sulphoaluminate cement and an alkali-activated cementitious material; the mineral admixture in the mineral admixture added Portland cement comprises one or a combination of more of silica fume, slag powder and fly ash; the sulphoaluminate cement comprises one or two of rapid hardening sulphoaluminate cement, high-strength sulphoaluminate cement and expansive sulphoaluminate cement; and the alkali-activated cementitious material comprises one of alkali-activated slag powder, and a combination of alkali-activated slag powder and fly ash.

### Claim 18 (depends on 11)

The emulsified asphalt cement-based coating according to claim 11, wherein the sand is one or more of river sand, machine-made sand or desalinated sea sand, with a particle size of 0.16 mm-2.36 mm.

### Claim 19 (depends on 11)

The emulsified asphalt cement-based coating according to claim 11, wherein the superplasticizer is one of polycarboxylate superplasticizer and naphthalene-based superplasticizer.

### Claim 20

A preparation method of an emulsified asphalt cement-based coating, comprising:
weighing an emulsified asphalt, a cementitious material, sand, water, biological calcium powder, calcium carbonate powder, trace elements, an acrylic emulsion and a superplasticizer;
adding the cementitious material, the biological calcium powder, the calcium carbonate powder, the trace elements and the polycarboxylate superplasticizer powder into a blender mixer, at rotational speed of 1000-1500 r/min, and continuously mixing for 4-8 min, uniformly mixing;
adding sand into mixer, adjusting the rotational speed to 500-1000 r/min, and mixing for 2-5 min, and standing for later use; and
adding the acrylic emulsion and the emulsified asphalt, uniformly mixing with water, putting into a high-speed stirrer at a speed of 200-500 r/min together with uniformly-mixed material and mixing for 5-10 min.