# US 2022/0317109 A1 · Method for the assessment of alkali-silica reactivity of aggregates and concrete mixtures

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0317109 A1
- Document ID: US20220317109A1
- Status: Published application
- Kind: A1
- Application number: 17/112,090
- Filed: 2020-12-04
- Published: 2022-10-06
- Earliest claimed: 2020-12-04
- Assignees: The United States Department of Transportation, Federal Highway Administration
- Inventors: Terence S Arnold; Chandni Balachandran; Jose F Munoz
- Web page: https://patentgrep.com/patent/US20220317109A1

## CPC

- G01N 33/383: {Concrete or cement}
- C04B 40/0032: {Controlling the process of mixing, e.g. adding ingredients in a quantity depending on a measured or desired value (B28C7/00 takes precedence)}
- C04B 40/0082: {making use of a rise in temperature, e.g. caused by an exothermic reaction}
- C04B 2111/2023: {Resistance against alkali-aggregate reaction}
- G01N: INVESTIGATING OR ANALYSING MATERIALS BY DETERMINING THEIR CHEMICAL OR PHYSICAL PROPERTIES (measuring or testing apparatus or processes other than immunoassay, involving enzymes or microorganisms C12M, C12Q)
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE

## Abstract

Chemical test methods for evaluating the alkali-silica reactivity (ASR) of an aggregate or an aggregate within a particular concrete job mix design by exposing the aggregate to a simplified system with the same or simulated long-term pore solution conditions is provided. ASR is a chemical reaction occurring between alkaline hydroxides within cement paste and certain types of amorphous silica found in mineral aggregates. Causing an accumulation of internal pressure within concrete structures due to the formation of a hygroscopic gel through the absorption of water, ASR leads to expansion and cracking of concrete. The present test method determines the reactivity index (RI) of a given aggregate, or an aggregate as it is to be used in a proposed concrete job mix design by determining the average concentrations of calcium, aluminum, and silicon across multiple tested samples, wherein the RI is the ratio of the concentrations of silicon to that of aluminum and calcium combined.

## Claims

### Claim 1

A chemical test method for assessing the likelihood of the formation of alkali-silica reaction gels in concrete comprising the steps of:
preparing a plurality of replicates for simulating a plurality of long-term pore conditions using a preselected aggregate;
heating a first portion of said plurality of replicates in a first oven for a period of time;
heating a second portion of said plurality of replicates in a second oven for said period of time
filtering the contents of each of said plurality of replicates after the expiry of said period of time;
measuring the concentrations of silicon, aluminum, and calcium in each of said filtered contents; and
calculating a reactivity index value using said measured concentrations of silicon, aluminum, and calcium that is indicative of said alkali-silica reactivity of said aggregate in each of said plurality of simulated long-term pore conditions.

### Claim 2 (depends on 1)

The method of claim 1, further comprising the preparation of said preselected aggregate for testing where said preselected aggregate is coarse, including the steps of:
crushing said preselected aggregate;
sieving said crushed aggregate and retaining those portions that are captured by #50 and #100 sieves;
washing and drying said retained crushed aggregate portions separately; and
homogenizing said retained aggregate portions by mixing them at a ratio of 1 part of said retained aggregate portion captured by said #100 sieve to 1.66 parts of said retained aggregate portion captured by said #50 sieve.

### Claim 3 (depends on 1)

The method of claim 1, wherein the preparation of each of said plurality of replicates further comprises:
selecting a suitable, non-reactive container;
adding a defined amount of calcium oxide to said container;
adding five grams of said preselected aggregate to said container;
adding a defined amount of a soluble alkali to said container; and
sealing said container.

### Claim 4 (depends on 3)

The method of claim 3, wherein said defined amount of calcium oxide is determined based on a pre-established testing chart; and
wherein said pre-established testing chart provides at least four different calcium oxide amounts, one each for said plurality of simulated long-term pore conditions.

### Claim 5 (depends on 4)

The method of claim 4, wherein said defined amount of said soluble alkali is 25 mL of 1 N sodium hydroxide.

### Claim 6 (depends on 5)

The method of claim 5, wherein at least three replicates are prepared for each of said at least four simulated long-term pore conditions; and
wherein said calculated reactivity index for each of said simulated pore conditions under test is the average of the individual calculated reactivity indexes for each of said at least three replicates for each of said at least four simulated long-term pore conditions.

### Claim 7 (depends on 6)

The method of claim 6, wherein said calculated reactivity index for each of said at least four simulated long-term pore conditions are compared to a pre-established chart to determine the likelihood of the formation of alkali-silica reaction gel in concrete for said aggregate.

### Claim 8 (depends on 1)

The method of claim 1, wherein said first portion of said plurality of replicates are heated in said first oven at 55°±2° C.

### Claim 9 (depends on 1)

The method of claim 1, wherein said second portion of said plurality of replicates are heated in said second oven at 80°±2° C.

### Claim 10 (depends on 1)

The method of claim 1, wherein said period of time said first and second portions of said plurality of replicates are heated in said first and second ovens is twenty-one days.

### Claim 11 (depends on 1)

The method of claim 1, wherein said filtering of said contents of each replicate is performed via vacuum filtration through a glass microfiber filter having a pore size smaller than 0.7 μm.

### Claim 12

A chemical test method for assessing the likelihood of the formation of alkali-silica reaction gels in defined concrete job mix comprising the steps of:
preparing a mixed aggregate for testing;
preparing at least three replicates for simulating the long-term pore conditions of said defined concrete job mix using said mixed aggregate;
heating said at least three replicates in an oven for a period of time;
filtering the contents of each of said at least three replicates after the expiry of said period of time;
measuring the concentrations of silicon, aluminum, and calcium in each of said filtered contents; and
calculating a reactivity index value that is indicative of said alkali-silica reactivity of said mixed aggregate in said defined concrete job mix.

### Claim 13 (depends on 12)

The method of claim 12, wherein said preparation of said mixed aggregate further comprises the steps of:
crushing the coarse portion of said mixed aggregate;
sifting said crushed aggregate and retaining those portions of that are captured by #50 and #100 sieves;
washing and drying said retained crushed aggregate portions separately; and homogenizing said retained aggregate portions by mixing them at a ratio of 1 part of said retained aggregate portion captured by said #100 sieve to 1.66 parts of said retained aggregate portion captured by said #50 sieve.

### Claim 14 (depends on 13)

The method of claim 13, wherein the preparation of each of said at least three replicates further comprises:
selecting a suitable, non-reactive container;
adding a calculated amount of calcium oxide to said container;
adding an amount of fine aggregate to said container as required to satisfy said defined concrete job mix based on five grams of homogenized coarse aggregate;
adding said five grams of said homogenized coarse aggregate to said container;
adding a defined amount of a soluble alkali to said container; and
sealing said container.

### Claim 15 (depends on 14)

The method of claim 14, wherein said amount of calcium oxide is calculated based on said concrete job mix, a cement mill report, and a calculated amount of calcium hydroxide in the ordinary portland cement paste in the cement mix called for in said cement mill report.

### Claim 16 (depends on 15)

The method of claim 15, wherein said defined amount of said soluble alkali is 25 mL of a solution containing alkali concentration of sodium hydroxide and potassium hydroxide corresponding to the alkali content specified in said cement mill report.

### Claim 17 (depends on 12)

The method of claim 12, wherein said at least three replicates are heated in said oven at 55° C. for twenty-one days.

### Claim 18 (depends on 12)

The method of claim 12, wherein said filtering of said contents of each replicate is performed via vacuum filtration through a glass microfiber filter having a pore size smaller than 0.7 μm.

### Claim 19 (depends on 12)

The method of claim 12 wherein said reactivity index value represents the ratio of the said measured concentrations of silicon to that of aluminum and calcium combined.

### Claim 20

A method for assessing the likelihood of the formation of alkali-silica reaction gels in concrete comprising the steps of:
preparing a plurality of replicates for simulating the long-term pore conditions of a concrete using a specified aggregate;
conducting an accelerated exposure of said aggregate to said long-term pore conditions for a defined period of time;
analyzing the contents of each of said plurality of replicates for the concentrations of silicon, aluminum, and calcium after said defined period of time;
calculating the reactivity index value for each of said plurality of replicates and averaging their values; and
wherein said averaged reactivity value greater than 0.45 is indicative of the likely formation of alkali-silica reaction gels in said concrete using said aggregate.