# US 2022/0295645 A1 · Method for optimized filling hole and manufacturing fine line on printed circuit board

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0295645 A1
- Document ID: US20220295645A1
- Status: Published application
- Kind: A1
- Application number: 17/376,537
- Filed: 2021-07-15
- Published: 2022-09-15
- Earliest claimed: 2021-03-11
- Assignees: Albert Yeh; Triallian Corporation
- Applicants: Triallian Corporation
- Inventors: Albert Yeh; Nick Yang
- Web page: https://patentgrep.com/patent/US20220295645A1

## CPC

- H05K 3/423: {characterised by electroplating method}
- H05K 3/427: {initial plating of through-holes in metal-clad substrates}
- C25D 3/38: of copper
- C25D 5/02: Electroplating of selected surface areas
- C25D 5/022: {using masking means}
- C25D 5/18: Electroplating using modulated, pulsed or reversing current
- C25D 5/56: of plastics
- C25D 7/00: Electroplating characterised by the article coated
- H05K 3/0047: {Drilling of holes}
- H05K 3/188: {by direct electroplating}
- H05K 3/421: {Blind plated via connections (H05K3/422, H05K3/423 and H05K3/425 take precedence)}
- H05K 3/4644: {by building the multilayer layer by layer, i.e. build-up multilayer circuits (making via holes in the insulating layers H05K3/0011; special circuit boards as base or core whereon the multilayer is built H05K3/4602)}
- C25D 5/34: Pretreatment of metallic surfaces to be electroplated
- H05K 2201/09563: Metal filled via
- H05K 2203/054: Continuous temporary metal layer over resist, e.g. for selective electroplating
- H05K: PRINTED CIRCUITS; CASINGS OR CONSTRUCTIONAL DETAILS OF ELECTRIC APPARATUS; MANUFACTURE OF ASSEMBLAGES OF ELECTRICAL COMPONENTS
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR

## Abstract

A method for optimized filling holes and manufacturing fine lines on a printed circuit board (PCB) carries out the two processes separately. The inner wall of the hole is metalized with reduced graphene oxide (rGO) and then electroplated to fill the hole with copper. The processes are individually performed and thus operating parameters are considered independently. As a result, the copper-plating fillings are evenly compact and the fine lines have square profiles.

## Claims

### Claim 1

A method for optimized filling holes on a printed circuit board, comprising steps of:
(a) providing a copper clad substrate including a prepreg layer overlaid with a copper foil and a first dry film laminated on the copper foil, in which a blind hole with an insulative inner wall is formed at a predetermined position and defines an upper opening, wherein the first dry film is patterned corresponding to the upper opening and insoluble in a non-alkaline solution;
(b) modifying the insulative inner wall of the blind hole with reduced graphene oxide (rGO);
(c) depositing copper in the blind hole through an electroplating process;
(d) removing the first dry film to expose the copper foil; and
(e) removing the exposed copper foil.

### Claim 2 (depends on 1)

The method of claim 1, wherein the blind hole of step (a) is formed by steps of:
drilling a hole in the copper clad substrate overlaid with a copper foil at a predetermined position before laminating the first dry film on the copper foil;
and patterning the first dry film corresponding to the upper opening to form the blind hole.

### Claim 3 (depends on 1)

The method of claim 1, wherein the blind hole of step (a) is formed by steps of:
drilling a hole in the copper clad substrate with a copper foil at a predetermined position;
laminating a second dry film on the copper foil and forming a circuit pattern corresponding to designed fine lines;
depositing copper in the circuit pattern through an electroplating process;
removing the second dry film before laminating the first dry film on the copper foil; and
patterning the first dry film corresponding to the upper opening to form the blind hole.

### Claim 4 (depends on 3)

The method of claim 3, wherein the electroplating process of the step (a) is a vertical PPR (Periodic Pulse Reverse) plating process.

### Claim 5 (depends on 1)

The method of claim 1, wherein the blind hole of step (a) is formed by steps of:
providing a copper clad substrate overlaid with copper foils on opposite surfaces thereof and drilling a through hole with a lower opening or a blind hole with a bottom at a predetermined position;
laminating a second dry film on the copper foils and patterning the second dry film corresponding to an edge of the lower opening or the bottom;
depositing copper on the edge of the lower opening or in the bottom through an electroplating process;
removing the second dry film before laminating the first dry film on the copper foil; and
patterning the first dry film corresponding to the upper opening to form the blind hole.

### Claim 6 (depends on 5)

The method of claim 5, wherein the electroplating process of the step (a) is a vertical PPR (Periodic Pulse Reverse) plating process.

### Claim 7 (depends on 5)

The method of claim 5, wherein the second dry film is also patterned corresponding to designed fine lines, and copper is also deposited in the circuit pattern through the electroplating process.

### Claim 8 (depends on 1)

The method of claim 1, wherein the first dry film of the step (a) is patterned to expose an edge of the copper foil around the upper opening, and copper is deposited on the edge of the upper opening in the step (c).

### Claim 9 (depends on 1)

The method of claim 1, wherein the blind hole of step (a) is formed by a step of:
drilling a hole in the copper clad substrate overlaid with the copper foil and laminated the first dry film on the copper foil at a predetermined position.

### Claim 10 (depends on 1)

The method of claim 1, wherein the step (b) comprises forming a polymer layer on the first dry film and the insulative wall of the blind hole, then modifying the polymer layer with graphene oxide (GO), and finally reducing the GO to form a reduced GO (rGO) layer.

### Claim 11 (depends on 1)

The method of claim 1, wherein the step (c) further comprises depositing copper on the rGO layer on the first dry film to form a surface copper layer.

### Claim 12 (depends on 1)

The method of claim 1, wherein the step (d) further comprises steps of:
removing the surface copper layer to expose the rGO layer on the first dry film; and
removing the rGO layer on the first dry film before removing the first dry film.

### Claim 13 (depends on 1)

The method of claim 1, wherein the step (e) further comprises steps of:
laminating a second dry film on the copper foil and forming an non-conductive pattern by masking area required to be conductive; and
removing the copper foil in the non-conductive pattern,
before removing the second dry film.

### Claim 14

A method for optimized filling holes and manufacturing fine lines on a printed circuit board, comprising steps of:
(a1) providing a copper clad substrate overlaid with a copper foil and drilling a hole at a predetermined position, wherein the hole has an upper opening with an insulative inner wall;
(a2) laminating a second dry film on the copper foil and forming a circuit pattern corresponding to designed fine lines;
(a3) depositing copper in the circuit pattern through an electroplating process;
(a4) removing the second dry film;
(a5) laminating the first dry film on the copper foil and patterning the first dry film corresponding to the upper opening to form a blind hole, wherein the first dry film is insoluble in a non-alkaline solution;
(b) modifying the insulative inner wall of the blind hole with reduced graphene oxide (rGO);
(c) depositing copper in the blind hole through an electroplating process;
(d) removing the first dry film; and
(e) removing exposed copper foil.

### Claim 15 (depends on 14)

The method of claim 14, wherein the step (a3) performs a vertical PPR (Periodic Pulse Reverse) plating process.

### Claim 16 (depends on 14)

The method of claim 14, wherein:
in step (a1), the copper clad substrate is overlaid with copper foils on opposite surfaces thereof and the hole is a through hole with a lower opening or a blind hole with a bottom at a predetermined position;
in step (a2), a second dry film is laminated on each of the copper foils and patterned corresponding to an edge of the lower opening or the bottom; and
in step (a3), copper is deposited on the edge of the lower opening or in the bottom through an electroplating process.

### Claim 17 (depends on 14)

The method of claim 14, wherein the first dry film of the step (a5) is patterned to expose an edge of the copper foil around the upper opening, and copper is deposited on the edge of the upper opening in the step (c).

### Claim 18 (depends on 14)

The method of claim 14, wherein the step (b) includes forming a polymer layer on the first dry film and the insulative wall of the blind hole, then modifying the polymer layer with graphene oxide (GO), and finally reducing the GO to form a reduced GO (rGO) layer.

### Claim 19 (depends on 14)

The method of claim 14, wherein the step (c) further comprises depositing copper on the rGO layer on the first dry film to form a surface copper layer.

### Claim 20 (depends on 19)

The method of claim 19, wherein the step (d) further comprises removing the surface copper layer to expose the rGO layer on the first dry film and then removing the rGO layer on the first dry film before removing the first dry film.