# US 2022/0285750 A1 · Process and its products for spent lithium-ion batteries treatment

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0285750 A1
- Document ID: US20220285750A1
- Status: Published application
- Kind: A1
- Application number: 17/443,818
- Filed: 2021-07-27
- Published: 2022-09-08
- Earliest claimed: 2021-03-08
- Assignees: Tsinghua University
- Applicants: Tsinghua University
- Inventors: Jinhui LI; Jiadong YU; Lili LIU
- Web page: https://patentgrep.com/patent/US20220285750A1

## CPC

- H01M 10/54: Reclaiming serviceable parts of waste accumulators
- C01G 53/42: containing alkali metals, e.g. LiNiO2
- C01G 53/82: Compounds containing nickel, with or without oxygen or hydrogen, and containing two or more other elements
- C22B 1/005: {Preliminary treatment of scrap (C22B1/02 - C22B1/26 take precedence)}
- C22B 3/165: {with organic acids}
- C22B 3/46: by substitution, e.g. by cementation
- C22B 7/005: {Separation by a physical processing technique only, e.g. by mechanical breaking}
- C22B 7/007: {by acid leaching}
- C22B 15/0067: {with acids or salts thereof}
- C22B 21/0023: {from waste materials}
- C22B 23/0415: {with acids or salt solutions except ammonium salts solutions}
- C22B 23/0469: {by chemical substitution, e.g. by cementation}
- C22B 26/12: Obtaining lithium
- H01M 4/485: of mixed oxides or hydroxides for inserting or intercalating light metals, e.g. LiTi2O4 or LiTi2OxFy (H01M4/505, H01M4/525 take precedence)
- H01M 4/525: of mixed oxides or hydroxides containing iron, cobalt or nickel for inserting or intercalating light metals, e.g. LiNiO2, LiCoO2 or LiCoOxFy
- H01M 10/052: Li-accumulators
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- C01P 2002/54: one element only
- Y02E 60/10: Energy storage using batteries
- Y02W 30/84: Recycling of batteries or fuel cells
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01G: COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts or peroxyacids C01B15/00; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium, or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds containing nitrogen, other non-metals and metal C01B21/082}; metal amides C01B21/092; nitrites C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; compounds having molecular sieve properties but not having base-exchange properties C01B37/00; compounds having molecular sieve and base-exchange properties, e.g. crystalline zeolites, C01B39/00; cyanides C01C3/08; salts of cyanamide C01C3/16; thiocyanates C01C3/20)
- C22B: PRODUCTION AND REFINING OF METALS (electrolytic C25); PRETREATMENT OF RAW MATERIALS
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION
- Y02W: CLIMATE CHANGE MITIGATION TECHNOLOGIES RELATED TO WASTEWATER TREATMENT OR WASTE MANAGEMENT

## Abstract

This invention discloses a process and its products for spent lithium-ion batteries treatment, which relates to the field of spent battery treatment technology. This process comprises: fully discharging spent lithium-ion batteries to obtain discharged spent lithium-ion batteries; crushing spent lithium-ion batteries to obtain crushed products of spent lithium-ion batteries; screening crushed products of spent lithium-ion batteries by screens to obtain an overflow and an underflow; sorting the overflow to obtain separator products, plastic products, iron products, copper foil products and aluminum foil products; mechanochemically activating the underflow to obtain activated products; acid leaching the activated products by degradable organic acid to obtain a mixture containing activated products and the organic acid leaching solution; filtering the mixture which contains the activated products and the organic acid leaching solution to obtain graphite as filter residues. Copper mud products and LiNi0.85Co0.1Al0.05O2 can be obtained after further treatments. This process can effectively recover recyclable resources in spent lithium-ion batteries, and reduce pollution of heavy metals.

## Claims

### Claim 1

A process of spent lithium-ion batteries treatment, wherein features comprise:
fully discharging spent lithium-ion batteries to obtain discharged spent lithium-ion batteries;
crushing said spent lithium-ion batteries to obtain said crushed products of spent lithium-ion batteries;
screening said crushed products of spent lithium-ion batteries by screens to obtain an overflow and an underflow;
sorting said overflow to obtain separator products, plastic products, iron products, copper foil products and aluminum foil products;
mechanochemically activating said underflow to obtain activated products;
acid leaching said activated products by degradable organic acid to obtain a mixture containing activated products and the organic acid leaching solution;
filtering the mixture which contains the activated products and the organic acid leaching solution to obtain graphite as filter residues.

### Claim 2 (depends on 1)

The process as claimed in claim 1, wherein features also comprise following steps:
putting said aluminum foil products into said organic acid leaching solution to conduct purification and transformation, to obtaining the mixture of flocculated pure copper mud products and purified leaching solution through displacement reaction;
filtering said mixture of flocculated pure copper mud products and purified leaching solution, then obtaining flocculated pure copper mud products as filter residues and purified leaching solution as filtrate.

### Claim 3 (depends on 2)

The process as claimed in claim 2, wherein features comprise:
adding cobalt acetate and nickelous acetate into said purified leaching solution to obtain primary intermediate products;
adding NaOH and buffer solution into said primary intermediate products, controlling pH value between 12±0.1, precipitating after fully stirring, then, obtaining a lithium-rich solution as filtrate, and Ni0.85Co0.1Al0.05(OH)2 as filter residues after solid-liquid separation;
adopting hydrothermal reaction for said Ni0.85Co0.1Al0.05(OH)2 to conduct secondary crystallization and precipitation, then, obtaining ternary precursor of lithium-ion batteries;
adding Na2CO3 into said lithium-rich solution, heating to the first setting temperature, and filtering while it is hot to obtain Li2CO3;
mixing said ternary precursor of lithium-ion batteries and Li2CO3 as setting ratio, then, obtaining LiNi0.85Co0.1Al0.05O2 after roasting for setting time at the second setting temperature.

### Claim 4 (depends on 1)

The process as claimed in claim 1, wherein features of fully discharging spent lithium-ion batteries to obtain discharged spent lithium-ion batteries comprise following steps:
putting said spent lithium-ion batteries into a NaCl—KCl solution which the mass percentage of solute is between 5%-10% to fully discharge for 40 h-60 h, thereby obtaining secondary intermediate products;
drying said secondary intermediate products to obtain said discharged spent lithium-ion batteries.

### Claim 5 (depends on 4)

The process as claimed in claim 4, wherein the step of drying said secondary intermediate products is accomplished in a fume cupboard by natural air drying for 40 h-60 h.

### Claim 6 (depends on 1)

The process as claimed in claim 1, wherein features of crushing spent lithium-ion batteries to obtain crushed products of spent lithium-ion batteries comprise following steps:
coarsely crushing said spent lithium-ion batteries by a shearing machine to obtain coarsely crushed spent lithium-ion batteries;
finely crushing said coarsely crushed spent lithium-ion batteries by a pulverizer to obtain said crushed products of spent lithium-ion batteries.

### Claim 7 (depends on 1)

The process as claimed in claim 1, wherein the range of mesh size is between 2 mm-6 mm during the step of screening said crushed products of spent lithium-ion batteries by screens to obtain the overflow and the underflow.

### Claim 8 (depends on 1)

The process as claimed in claim 1, wherein the screen is the circle vibrating sieve during the step of crushing spent lithium-ion batteries to obtain crushed products of spent lithium-ion batteries.

### Claim 9 (depends on 1)

The process as claimed in claim 1, wherein, during the process of sorting said overflow to obtain separator products, plastic products, iron products, copper foil products and aluminum foil products,
said separator products and plastic products are obtained by pneumatic separation;
said iron products are obtained by magnetic selection;
said copper foil products are obtained by color sorting;
rest products after said pneumatic separation, magnetic selection and color sorting are aluminum foil products.

### Claim 10 (depends on 9)

The process as claimed in claim 9, wherein said magnetic selection is conducted repeatedly.

### Claim 11 (depends on 1)

The process as claimed in claim 1, wherein the step of mechanochemically activating of said underflow is conducted by a planetary ball mill during the process of said mechanochemically activating the underflow to obtain activated products.

### Claim 12 (depends on 11)

The process as claimed in claim 11, wherein the duration of grinding the underflow in said planetary ball mill is between 1 h-2 h.

### Claim 13 (depends on 3)

The process as claimed in claim 3, wherein the duration of said full precipitation is between 1 h-4 h during the process of adding NaOH and buffer solution into primary intermediate products, controlling pH between 12±0.1, precipitating after full stirring and obtaining a lithium-rich solution as filtrate, and Ni085Co0.1Al0.05(OH)2 as filter residues after solid-liquid separation.

### Claim 14 (depends on 3)

The process as claimed in claim 3, wherein the range of said first setting temperature is between 90° C.-100° C. during the process of adding excessive Na2CO3 into the lithium-rich solution, heating to the first setting temperature, and filtering while it is hot to obtain Li2CO3.

### Claim 15 (depends on 3)

The process as claimed in claim 3, wherein the range of said second setting temperature is between 800° C.-900° C. during the process of mixing said ternary precursor of lithium-ion batteries and Li2CO3 as setting ratio and obtaining LiNi0.85Co0.1Al0.05O2 after roasting setting time at the second setting temperature;

### Claim 16 (depends on 3)

The process as claimed in claim 3, wherein the range of said second setting temperature is between 800° C.-900° C. during the process of mixing said ternary precursor of lithium-ion batteries and Li2CO3 as setting ratio and obtaining LiNi0.85Co0.1Al0.05O2 after roasting setting time at the second setting temperature.

### Claim 17 (depends on 3)

The process as claimed in claim 3, wherein the ratio range of maxing said ternary precursor of lithium-ion batteries and Li2CO3 is 1:(1-1.10).

### Claim 18 (depends on 3)

The process as claimed in claim 3, wherein said mixing is accomplished by grinding during the process of mixing said ternary precursor of lithium-ion batteries and Li2CO3 as setting ratio and obtaining LiNi0.85Co0.1Al0.05O2 after roasting for setting time at the second temperature.

### Claim 19

Products of spent lithium-ion batteries treatment as wherein features comprise one or several of separator products, plastic products, iron products, copper foil products and aluminum foil products.

### Claim 20 (depends on 19)

Products of the process as claimed in claim 19, wherein features comprise:
putting said aluminum foil products into organic acid for purification and transformation to obtain the mixture of flocculated pure copper mud products and purified leaching solution;
filtering said mixture of flocculated pure copper mud products and purified leaching solution, then obtaining flocculated pure copper mud products as filter residues and purified leaching solution as filtrate;
adding cobalt acetate and nickelous acetate into said purified leaching solution to obtain primary intermediate products;
adding NaOH and buffer solution into the primary intermediate products, controlling pH value between 12±0.1, precipitating after full stirring, and obtaining a lithium-rich solution as filtrate, and Ni0.85Co0.1Al0.05(OH)2 as filter residues after solid-liquid separation;
adopting hydrothermal reaction to conduct secondary crystallization and precipitation for said Ni0.85Co0.1Al0.05(OH)2, then, obtaining ternary precursor of lithium-ion batteries;
adding excessive Na2CO3 into the lithium-rich solution, heating to the first setting temperature, and filtering while it is hot to obtain Li2CO3;
mixing said ternary precursor of lithium-ion batteries and Li2CO3 as setting ratio, then, obtaining LiNi0.85Co0.1Al0.05O2 after roasting setting time at the second setting temperature.
