# US 2022/0282404 A1 · Polyamide 56 fibre with low boiling water shrinkage rate, preparation method therefor, and application thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0282404 A1
- Document ID: US20220282404A1
- Status: Published application
- Kind: A1
- Application number: 17/637,093
- Filed: 2020-01-15
- Published: 2022-09-08
- Earliest claimed: 2019-08-22
- Applicants: Cathay Biotech Inc.; CIBT America Inc.
- Inventors: Chaoxu SUN; Xiucai LIU
- Web page: https://patentgrep.com/patent/US20220282404A1

## CPC

- D01F 6/60: from polyamides (from polyamino acids or polypeptides D01F6/68)
- C08G 69/28: Preparatory processes
- D01D 5/092: in shafts or chimneys
- D02G 1/20: Combinations of two or more of the above-mentioned operations or devices; After-treatments for fixing crimp or curl
- D10B 2331/02: polyamides (D10B2331/08 takes precedence)
- D01F: CHEMICAL FEATURES IN THE MANUFACTURE OF ARTIFICIAL FILAMENTS, THREADS, FIBRES, BRISTLES OR RIBBONS; APPARATUS SPECIALLY ADAPTED FOR THE MANUFACTURE OF CARBON FILAMENTS
- C08G: MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
- D01D: MECHANICAL METHODS OR APPARATUS IN THE MANUFACTURE OF ARTIFICIAL FILAMENTS, THREADS, FIBRES, BRISTLES OR RIBBONS
- D02G: CRIMPING OR CURLING FIBRES, FILAMENTS, THREADS, OR YARNS; YARNS OR THREADS
- D10B: INDEXING SCHEME ASSOCIATED WITH SUBLASSES OF SECTION D, RELATING TO TEXTILES

## Abstract

The present invention relates to the technical field of polyamide materials, and provides a polyamide 56 pre-oriented yarn and a polyamide 56 draw textured yarn with a low shrinkage in boiling water, a process for producing the same and a use thereof. The raw materials for producing the polyamide 56 fiber comprise 1,5-pentane diamine and adipic acid, or a polyamide 56 resin obtained by polymerizing 1,5-pentane diamine monomer and adipic acid monomer; wherein the polyamide 56 fiber has a shrinkage in boiling water of 9% or less, wherein the polyamide 56 fiber comprises a polyamide 56 pre-oriented yarn with a low shrinkage in boiling water and a polyamide 56 draw textured yarn with a low shrinkage in boiling water. The polyamide 56 fiber has good mechanical properties, dyeing uniformity and dimensional stability. The process for producing the polyamide 56 fiber does not require modification to existing equipments for texturing polyamide fibers and thus reduces production costs.

## Claims

### Claim at position 1

1-11. (canceled)

### Claim 12

A polyamide 56 fiber, characterized in that raw materials for producing the polyamide 56 fiber comprise 1,5-pentane diamine and adipic acid, or a polyamide 56 resin obtained by polymerizing 1,5-pentane diamine monomer and adipic acid monomer; wherein the polyamide 56 fiber has a shrinkage in boiling water of 9% or less.

### Claim 13 (depends on 12)

The polyamide 56 fiber according to claim 12, characterized in that the polyamide 56 fiber comprises a polyamide 56 pre-oriented yam with a low shrinkage in boiling water and a polyamide 56 draw textured yarn with a low shrinkage in boiling water, and/or
the polyamide 56 resin has an oligomer content of 1.2 wt % or less, and preferably 0.8 wt % or less;
wherein the oligomer is selected from the following structures:
wherein n1 and n2 are respectively selected from integers of 1-8, m1 and m2 are 4, preferably, n1 and n2 are respectively selected from integers of 1-6; more preferably, n1 and n2 each independently are integers of 1-5; and further preferably, n1 is 1, 2, 3 or 4; and n2 is 1, 2, 3, 4 or 5; and/or
the polyamide 56 fiber comprises a bright fiber, a semi-dull fiber and a fully-dull polyamide 56 fiber.

### Claim 14 (depends on 13)

The polyamide 56 fiber according to claim 13, characterized in that the polyamide 56 pre-oriented yarn has a shrinkage in boiling water of 9% or less, further preferably 8% or less, and still further preferably 7% or less; and/or
the polyamide 56 pre-oriented yarn has a fineness of 10-300 dtex, preferably 20-200 dtex, further preferably 30-100 dtex, and still further preferably 50-80 dtex; and/or
the polyamide 56 pre-oriented yam has a break strength of 3.0-4.5 cN/dtex, preferably 3.3-4.3 cN/dtex, further preferably 3.5-4.1 cN/dtex, and still further preferably 3.7-3.9 cN/dtex; and/or
the polyamide 56 pre-oriented yam has an elongation at break of 60-90%, preferably 65-85%, further preferably 70-80%, and still further preferably 73-78%; and/or
the polyamide 56 pre-oriented yarn has a dyeing uniformity (grey scale) of grade 3 or more, preferably grade 3.5 or more, further preferably grade 4.0 or more, and still further preferably grade 4.5 or more.

### Claim 15 (depends on 13)

The polyamide 56 fiber according to claim 13, characterized in that the polyamide 56 draw textured yarn has a shrinkage in boiling water of 8% or less, further preferably 7% or less, and still further preferably 6% or less; and/or
the polyamide 56 draw textured yarn has a fineness of 10-200 dtex, preferably 20-100 dtex, further preferably 30-80 dtex, and still further preferably 40-60 dtex; and/or
the polyamide 56 draw textured yarn has a break strength of 3.5-5.5 cN/dtex, preferably 3.8-5.0 cN/dtex, further preferably 4.0-4.7 cN/dtex, and still further preferably 4.3-4.5 cN/dtex; and/or
the polyamide 56 draw textured yarn has an elongation at break of 20-50%, preferably 25-45%, further preferably 30-40%, and still further preferably 33-36%; and/or
the polyamide 56 draw textured yarn has a crystallinity of 60% or more, preferably 63% or more, further preferably 66% or more, and still further preferably 68% or more; and/or
the polyamide 56 draw textured yarn has an orientation degree of 60% or more, preferably 65% or more, further preferably 70% or more, and still further preferably 73% or more; and/or
the polyamide 56 draw textured yarn has a dyeing uniformity (grey scale) of grade 3 or more, preferably grade 3.5 or more, further preferably grade 4.0 or more, and still further preferably grade 4.5 or more.

### Claim 16 (depends on 13)

The polyamide 56 fiber according to claim 13, characterized in that the polyamide 56 draw textured yarn has a shrinkage in boiling water of 2-8%, a break strength of 3.5-5.5 cN/dtex, an elongation at break of 20-50%, a crystallinity of 60-80%, or an orientation degree of 60-90%.

### Claim 17

A process for producing a polyamide 56 pre-oriented yarn, characterized in that the process comprises the following steps:
(1) polymerizing 1,5-pentane diamine and adipic acid to form a polyamide 56 melt; or heating a polyamide 56 resin into a molten state with a screw to form a polyamide 56 melt;
(2) conveying the polyamide 56 melt into a spinning box through a melt pipeline, precisely metering the melt with a metering pump, and then injecting it into a spinning assembly, and extruding it through a spinneret orifice; and
(3) cooling, spinning finishing, drawing and winding the extruded as-spun fiber to obtain the polyamide 56 pre-oriented yarn.

### Claim 18 (depends on 17)

The process according to claim 17, characterized in that
in step (1), the polyamide 56 resin has a relative viscosity of 2.4-2.8, and preferably 2.5-2.7; and the polyamide 56 resin has an oligomer content of 1.2 wt % or less, and preferably 0.8 wt % or less; and/or
the polyamide 56 resin has a moisture content of 600-1200 ppm, and preferably 800-1000 ppm; and/or
the polyamide 56 resin has a number average molecular weight of 15,000-22,000, and preferably 18,000-20,000, or has a molecular weight distribution of 1.0-2.0, and preferably 1.2-1.8; and/or the screw is heated with four zones, wherein the temperature of a first zone is 245-260° C., and preferably 250-255° C.; the temperature of a second zone is 260-275° C., and preferably 265-270° C.; the temperature of a third zone is 275-285° C., and preferably 278-283° C.; and the temperature of a fourth zone is 280-285° C., and preferably 282-284° C.

### Claim 19 (depends on 17)

The process according to claim 17, characterized in that
in Step (2), the temperature of the box is 275-285° C., and preferably 280-283° C.; the pressure of the assembly is 13-20 MPa, and preferably 15-18 MPa; and/or
in Step (3), the cooling comprises cooling with cross air blow side air blow or cross air blow, preferably cooling with cross air blow; and an air speed is preferably 0.2-0.6 m/s, and more preferably 0.3-0.5 m/s; and/or an air temperature is 18-25° C., preferably 20-23° C., and more preferably 21-22° C.; and/or
the spinning finishing is conducted with an oil roll; and an oil pick up is 0.2-0.8 wt %, preferably 0.3-0.7 wt %, and more preferably 0.4-0.5 wt %; and/or
a winding speed is 4,000-5,500 m/min, preferably 4,300-5,000 m/min, and more preferably 4,500-4,800 m/min.

### Claim 20 (depends on 17)

The process according to claim 17, characterized in that the polyamide 56 resin has an oligomer content of 1.2 wt % or less, and preferably 0.8 wt % or less;
wherein the oligomer is selected from the following structures:
wherein n1 and n2 are respectively selected from integers of 1-8, m1 and m2 are 4, preferably, n1 and n2 are respectively selected from integers of 1-6; more preferably, n1 and n2 each independently are integers of 1-5; and further preferably, n1 is 1, 2, 3 or 4; and n2 is 1, 2, 3, 4 or 5.

### Claim 21 (depends on 17)

The process according to claim 17, characterized in that the polyamide 56 pre-oriented yarn has a shrinkage in boiling water of 9% or less, further preferably 8% or less, and still further preferably 7% or less; and/or
the polyamide 56 pre-oriented yarn has a fineness of 10-300 dtex, preferably 20-200 dtex, further preferably 30-100 dtex, and still further preferably 50-80 dtex; and/or
the polyamide 56 pre-oriented yarn has a break strength of 3.0-4.5 cN/dtex, preferably 3.3-4.3 cN/dtex, further preferably 3.5-4.1 cN/dtex, and still further preferably 3.7-3.9 cN/dtex; and/or
the polyamide 56 pre-oriented yarn has an elongation at break of 60-90%, preferably 65-85%, further preferably 70-80%, and still further preferably 73-78%; and/or
the polyamide 56 pre-oriented yarn has a dyeing uniformity (grey scale) of grade 3 or more, preferably grade 3.5 or more, further preferably grade 4.0 or more, and still further preferably grade 4.5 or more.

### Claim 22

A process for producing the polyamide 56 draw textured yarn, characterized in that the process comprises the following steps:
a) directing the polyamide 56 pre-oriented yarn to a first roller with a guide; conveying it through a twist stopper, and thermally drawing the pre-oriented yarn in a first hot box;
b) cooling and setting the pre-oriented yarn with a cooling plate; conveying it through a false twister, a second roller, and an interlacing device; and spinning finishing it with an oil roll; and
c) winding the pre-oriented yarn to obtain a polyamide 56 draw textured yarn.

### Claim 23 (depends on 22)

The process according to claim 22, characterized in that
a thermal drawing ratio is 1.1-1.5, preferably 1.15-1.4, and more preferably 1.2-1.3; and/or, a thermal drawing temperature is 150-220° C., preferably 160-200° C., and more preferably 170-180° C.; and/or
a speed ratio D/Y of the false twister is 1.3-2.2, preferably 1.5-2.0, and more preferably 1.7-1.8; and/or
a pressure of compressed air in the interlacing device is 0.3-1.5 MPa, preferably 0.5-1.2 MPa, and more preferably 0.7-0.8 MPa; and/or
a winding speed is 300-800 m/min, preferably 400-700 m/min, and more preferably 500-600 m/min; and/or a winding overfeed is 2-8%, preferably 3-6%, and more preferably 4-5%.

### Claim 24 (depends on 22)

The process according to claim 22, characterized in that the polyamide 56 draw textured yarn has a shrinkage in boiling water of 8% or less, further preferably 7% or less, and still further preferably 6% or less; and/or
the polyamide 56 draw textured yarn has a fineness of 10-200 dtex, preferably 20-100 dtex, further preferably 30-80 dtex, and still further preferably 40-60 dtex; and/or
the polyamide 56 draw textured yarn has a break strength of 3.5-5.5 cN/dtex, preferably 3.8-5.0 cN/dtex, further preferably 4.0-4.7 cN/dtex, and still further preferably 4.3-4.5 cN/dtex; and/or
the polyamide 56 draw textured yarn has an elongation at break of 20-50%, preferably 25-45%, further preferably 30-40%, and still further preferably 33-36%; and/or
the polyamide 56 draw textured yarn has a crystallinity of 60% or more, preferably 63% or more, further preferably 66% or more, and still further preferably 68% or more; and/or
the polyamide 56 draw textured yarn has an orientation degree of 60% or more, preferably 65% or more, further preferably 70% or more, and still further preferably 73% or more; and/or
the polyamide 56 draw textured yarn has a dyeing uniformity (grey scale) of grade 3 or more, preferably grade 3.5 or more, further preferably grade 4.0 or more, and still further preferably grade 4.5 or more.

### Claim 25 (depends on 22)

The process according to claim 22, characterized in that the polyamide 56 draw textured yarn has a shrinkage in boiling water of 2-8%, a break strength of 3.5-5.5 cN/dtex, an elongation at break of 20-50%, a crystallinity of 60-80%, and an orientation degree of 60-90%.

### Claim 26 (depends on 12)

Use of the polyamide 56 fiber according to claim 12 in knitted or woven fabrics.