# US 2022/0282360 A1 · High formability steel sheet for the manufacture of lightweight structural parts and manufacturing process

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0282360 A1
- Document ID: US20220282360A1
- Status: Published application
- Kind: A1
- Application number: 17/751,615
- Filed: 2022-05-23
- Published: 2022-09-08
- Earliest claimed: 2017-04-21
- Assignees: ArcelorMittal
- Applicants: ArcelorMittal
- Inventors: Frédéric BONNET; Manuel BOBADILLA; Bertrand BELE; Valérie DAESCHLER
- Web page: https://patentgrep.com/patent/US20220282360A1

## CPC

- C22C 38/14: containing titanium or zirconium
- C21D 8/0215: {Rapid solidification; Thin strip casting}
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/08: containing nickel {(C22C38/105 takes precedence)}
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/32: with boron
- C21D 2211/001: Austenite
- C21D 2211/004: Dispersions; Precipitations
- C21D 2211/005: Ferrite
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)

## Abstract

A steel sheet has a composition comprising, by weight: 0.010%≤C≤0.080%, 0.06%≤Mn≤3%, Si≤1.5%, 0.005%≤Al≤1.5%, S≤0.030%, P≤0.040%, Ti and B such that: 3.2%≤Ti≤7.5% and (0.45×Ti) −1.35≤B≤(0.45×Ti) −0.43, optionally Ni≤1%, Mo≤1%, Cr≤3%, Nb≤0.1%, V≤0.1%, the remainder being iron and unavoidable impurities resulting from the smelting. The steel sheet has a structure consisting of ferrite, at most 10% of austenite, and precipitates comprising eutectic precipitates of TiB2, the volume fraction of TiB2 precipitates with respect to the whole structure being of at least 9%, the proportion of TiB2 precipitates having a surface area lower than 8 μm2 being of at least 96%.

## Claims

### Claim 1

A process for manufacturing a steel sheet, the process comprising the following successive steps:
providing a steel having a composition comprising, by weight percent:
0.010%≤C≤0.080%,
0.06%≤Mn≤3%,
Si≤1.5%,
0.005%≤Al≤1.5%,
S≤0.030%,
P≤0.040%,
Ti and B such that:
3.2%≤Ti≤7.5%,
(0.45×Ti)−1.35≤B≤(0.45×Ti)−0.43, and
optionally one or more elements chosen amongst:
Ni≤1%,
Mo≤1%,
Cr≤3%,
Nb≤0.1%,
V≤0.1%, and
a remainder being iron and unavoidable impurities; and
casting the steel to form a semi-product, with a casting temperature lower than or equal to Lliquidus+40° C., Lliquidus designating a liquidus temperature of the steel, the semi-product being cast in a form of a thin semi-product having a thickness of at most 110 mm, the steel being solidified during the casting with a solidification rate comprised between 0.03 cm/s and 5 cm/s at every location of the semi-product.

### Claim 2 (depends on 1)

The process according to claim 1, wherein the semi-product is cast in a form of a thin slab having a thickness lower than or equal to 110 mm.

### Claim 3 (depends on 1)

The process according to claim 1, wherein the semi-product is cast in a form of a thin slab having a thickness lower than or equal to 70 mm.

### Claim 4 (depends on 2)

The process according to claim 2, wherein the semi-product is cast by compact strip production.

### Claim 5 (depends on 1)

The process according to claim 1, wherein the semi-product is cast in a form of a thin strip having a thickness lower than or equal to 6 mm, the solidification rate being comprised between 0.2 cm/s and 5 cm/s at every location of the semi-product.

### Claim 6 (depends on 5)

The process according to claim 5, wherein the semi-product is cast by direct strip casting between counter-rotating rolls.

### Claim 7 (depends on 1)

The process according to claims 1, further comprising, after casting and solidification, hot-rolling the semi-product, to obtain a hot-rolled steel sheet.

### Claim 8 (depends on 7)

The process according to claim 7, wherein between casting and hot-rolling, a temperature of the semi-product remains higher than 700° C.

### Claim 9 (depends on 7)

The process according to claim 7, further comprising before the hot-rolling, de-scaling the semi-product at a temperature of at least 1050° C.

### Claim 10 (depends on 7)

The process according to claim 7, further comprising after the hot-rolling, cold-rolling the hot-rolled steel sheet, to obtain a cold-rolled steel sheet having a thickness lower than or equal to 2 mm.

### Claim 11 (depends on 1)

The process according to claim 1, wherein the titanium, boron and manganese contents are such that:
(0.45×Ti)−1.35≤B≤(0.45−Ti)−0.43
and (0.45×Ti)−1.35≤B≤(0.45×Ti)−(0.261×Mn)−0.414.

### Claim 12 (depends on 1)

The process according to claim 1, wherein the titanium and boron contents are such that:
(0.45×Ti)−1.35≤B≤(0.45×Ti)−0.50.

### Claim 13 (depends on 1)

The process according to claim 1, wherein the composition is such that 0.010%≤C≤0.050%.

### Claim 14 (depends on 1)

The process according to claim 1, wherein the composition is such that 0.005%≤Al≤1.3%.

### Claim 15 (depends on 1)

The process according to claim 1, wherein the steel sheet has a structure consisting of ferrite, at most 10% of austenite, and precipitates, said precipitates comprising eutectic precipitates of TiB2, a volume fraction of TiB2 precipitates with respect to the whole structure being at least 9%, a percentage of TiB2 precipitates having a surface area lower than 8 μm2 being at least 96%.

### Claim 16 (depends on 15)

The process according to claim 15, wherein a percentage of TiB2 precipitates having a surface area lower than 3 μm2 is at least 80%.

### Claim 17 (depends on 15)

The process according to claim 15, wherein a percentage of TiB2 precipitates having a surface area lower than 25 μm2 is 100%.

### Claim 18 (depends on 15)

The process according to claim 15, wherein in a core region of the steel sheet, a percentage of TiB2 precipitates having a surface area lower than 8 μm2 is at least 96%.

### Claim 19 (depends on 15)

The process according to claim 15, wherein said steel sheet comprises TiC precipitates with a volume fraction of 0.5% or lower.

### Claim 20 (depends on 15)

The process according to claim 15, wherein the steel sheet comprises no Fe2B precipitates.

### Claim 21 (depends on 1)

The process according to claim 1, wherein the steel sheet has a Charpy energy Kcv of at least 25 J/cm2 at −40° C.

### Claim 22 (depends on 1)

The process according to claim 1, wherein the steel sheet has a content in free Ti of at least 0.95% and less than 3%.