# US 2022/0281769 A1 · Chemically strengthened glass and manufacturing method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0281769 A1
- Document ID: US20220281769A1
- Status: Published application
- Kind: A1
- Application number: 17/652,543
- Filed: 2022-02-25
- Published: 2022-09-08
- Earliest claimed: 2021-02-26
- Assignees: AGC Inc.
- Applicants: Agc Inc.
- Inventors: Kaname SEKIYA; Yusuke FUJIWARA
- Web page: https://patentgrep.com/patent/US20220281769A1

## CPC

- C03C 21/002: {to perform ion-exchange between alkali ions (C03C21/005 takes precedence)}
- C03C 3/083: containing aluminium oxide or an iron compound
- C03C 3/095: containing rare earths
- C03C 4/18: for ion-sensitive glass
- C03C 2204/00: Glasses, glazes or enamels with special properties
- C03C: CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS

## Abstract

The present invention relates to a chemically strengthened glass having a thickness t (mm), in which a first-order derivative CSx′ of a stress value CSx (MPa) is −4.7 or larger in a range of CSx≥0 in a profile of the stress value CSx (MPa), in which the stress value CSx (MPa) is a function of depth×(μm) from a glass surface, and in which the stress value CSx (MPa) is measured by a scattered light photoelastic stress meter, and a manufacturing method thereof.

## Claims

### Claim 1

A chemically strengthened glass having a thickness t (mm), wherein a first-order derivative CSx′ of a stress value CSx (MPa) is −4.7 or larger in a range of CSx≥0 in a profile of the stress value CSx (MPa),
wherein the stress value CSx (MPa) is a function of depth×(μm) from a glass surface, and
wherein the stress value CSx (MPa) is measured by a scattered light photoelastic stress meter.

### Claim 2 (depends on 1)

The chemically strengthened glass according to claim 1, wherein in the profile of the stress value CSx, a second-order derivative CSx″ of the stress value CSx satisfies CSx″≤0.050.

### Claim 3 (depends on 1)

The chemically strengthened glass according to claim 1, wherein a second-order derivative CSx″ of the stress value CSx is larger than 0.

### Claim 4 (depends on 1)

The chemically strengthened glass according to claim 1, wherein the first-order derivative CSx′ of the stress value CSx is 0 or smaller.

### Claim 5 (depends on 1)

The chemically strengthened glass according to claim 1, wherein in the profile of the stress value CSx (MPa), a stress value CS0 at a glass outermost surface is 300 MPa or smaller.

### Claim 6 (depends on 1)

The chemically strengthened glass according to claim 1, wherein a maximum tensile stress CT2 (MPa) satisfies the following inequality:
CT2≤19.5/(t/2−DOL/1,000)
where t (mm) is the thickness and DOL (μm) is a compressive stress layer depth.

### Claim 7 (depends on 1)

The chemically strengthened glass according to claim 1, wherein a maximum stress value CS90 at a depth 90 (μm) from a glass surface satisfies the following inequality:
CS90/{CT2×(t−2×DOL/1,000)}/t≥1.62
where t (mm) is the thickness, CT2 (MPa) is a tensile stress and DOL (μm) is a compressive stress layer depth.

### Claim 8 (depends on 1)

The chemically strengthened glass according to claim 1, wherein:
the chemically strengthened glass is a chemically strengthened glass obtained by a chemical strengthening of two or more steps; and
a maximum tensile stress CT2 (MPa) of the chemically strengthened glass is 50% to 99% of a maximum tensile stress CT1 (MPa) of a chemically strengthened glass obtained after a first-stage chemical strengthening of the chemical strengthening of two or more steps.

### Claim 9 (depends on 1)

The chemically strengthened glass according to claim 1, wherein a base composition of the chemically strengthened glass comprises, as represented by mol % based on oxides,
SiO2 of 52% to 75%;
Al2O3 of 8% to 20%;
Li2O of 5% to 16%; and
Na2O of 8% or smaller.

### Claim 10

A manufacturing method for a chemically strengthened glass, the method comprising:
performing a first ion exchange by immersing a lithium-containing glass in a first molten salt composition containing sodium ions; and
performing a second ion exchange by immersing the lithium-containing glass obtained after the first ion exchange in a second molten salt composition containing potassium ions and lithium ions, wherein:
a concentration of a sodium nitrate in the first molten salt composition is higher than 50 mass %; and
in the second molten salt composition a concentration of a potassium nitrate is 85 mass % or higher and a ratio of a mass of sodium ions to a mass of lithium ions represented by a mass ratio of (sodium ions)/(lithium ions) is 0 or larger and 15 or smaller.

### Claim 11 (depends on 10)

The manufacturing method for a chemically strengthened glass according to claim 10, wherein the second molten salt composition contains a sodium nitrate of higher than 0 mass % and 5 mass % or lower.

### Claim 12 (depends on 10)

The manufacturing method for a chemically strengthened glass according to claim 10, wherein the second molten salt composition contains a lithium nitrate of 0.1 mass % or higher and 10 mass % or lower.

### Claim 13 (depends on 10)

The manufacturing method for a chemically strengthened glass according to claim 10, wherein in the first ion exchange the first molten salt composition has a temperature of 360° C. or higher and 450° C. or lower.

### Claim 14 (depends on 13)

The manufacturing method for a chemically strengthened glass according to claim 13, wherein in the first ion exchange the lithium-containing glass is immersed in the first molten salt composition for 0.5 hour or longer and 12 hours or shorter.

### Claim 15 (depends on 10)

The manufacturing method for a chemically strengthened glass according to claim 10, wherein in the second ion exchange the second molten salt composition has a temperature of 360° C. or higher and 450° C. or lower.

### Claim 16 (depends on 15)

The manufacturing method for a chemically strengthened glass according to claim 15, wherein in the second ion exchange the lithium-containing glass obtained after the first ion exchange is immersed in the second molten salt composition for an immersion time t2 (min) that satisfies the following inequality:
−0.38 T+173<t2<−1.4 T+720
where T (° C.) is the temperature of the second molten salt composition.

### Claim 17 (depends on 10)

The manufacturing method for a chemically strengthened glass according to claim 10, wherein the lithium-containing glass is chemically strengthened so that a maximum tensile stress CT2 (MPa) of the chemically strengthened glass obtained after the second ion exchange becomes 50% to 99% of a maximum tensile stress CT1 (MPa) of the chemically strengthened glass obtained after the first ion exchange.

### Claim 18 (depends on 10)

The manufacturing method for a chemically strengthened glass according to claim 10, wherein a maximum tensile stress CT1 (MPa) of the chemically strengthened glass obtained after the first ion exchange satisfies the following inequality:
CT1>17.5/(t/2−DOL/1,000)
where t is a thickness of the chemically strengthened glass and DOL (μm) is a compressive stress layer depth.

### Claim 19 (depends on 10)

The manufacturing method for a chemically strengthened glass according to claim 10, wherein the lithium-containing glass comprises, as represented by mol % based on oxides,
SiO2 of 52% to 75%;
Al2O3 of 8% to 20%;
Li2O of 5% to 16%; and
Na2O of 8% or smaller.

### Claim 20 (depends on 10)

The manufacturing method for a chemically strengthened glass according to claim 10, wherein the second molten salt composition contains a silicic acid.

### Claim 21 (depends on 10)

The manufacturing method for a chemically strengthened glass according to claim 10, wherein the second molten salt composition contains a carbonate.

### Claim 22

A manufacturing method for a chemically strengthened glass, the method comprising:
performing a first ion exchange by immersing a lithium-containing glass in a first molten salt composition containing sodium ions; and
performing a second ion exchange by immersing the lithium-containing glass obtained after the first ion exchange in a second molten salt composition containing potassium ions and lithium ions, wherein:
the lithium-containing glass is chemically strengthened so that a maximum tensile stress CT2 (MPa) of the chemically strengthened glass obtained after the second ion exchange becomes 50% to 99% of a maximum tensile stress CT1 (MPa) of the chemically strengthened glass obtained after the first ion exchange.

### Claim 23 (depends on 22)

The manufacturing method for a chemically strengthened glass according to claim 22, wherein:
a concentration of a sodium nitrate in the first molten salt composition is higher than 50 mass %; and
a concentration of a potassium nitrate in the second molten salt composition is 85 mass % or higher.

### Claim 24 (depends on 22)

The manufacturing method for a chemically strengthened glass according to claim 22, wherein a second molten salt composition contains a sodium nitrate of higher than 0 mass % and 5 mass % or lower.

### Claim 25 (depends on 22)

The manufacturing method for a chemically strengthened glass according to claim 22, wherein the second molten salt composition contains a lithium nitrate of 0.1 mass % or higher and 10 mass % or lower.

### Claim 26 (depends on 22)

The manufacturing method for a chemically strengthened glass according to claim 22, wherein in the first ion exchange the first molten salt composition has a temperature of 360° C. or higher and 450° C. or lower.

### Claim 27 (depends on 26)

The manufacturing method for a chemically strengthened glass according to claim 26, wherein in the first ion exchange the lithium-containing glass is immersed in the first molten salt composition for 0.5 hour or longer and 12 hours or shorter.

### Claim 28 (depends on 22)

The manufacturing method for a chemically strengthened glass according to claim 22, wherein in the second ion exchange the second molten salt composition has a temperature of 360° C. or higher and 450° C. or lower.

### Claim 29 (depends on 28)

The manufacturing method of a chemically strengthened glass according to claim 28, wherein in the second ion exchange the lithium-containing glass obtained after the first ion exchange is immersed in the second molten salt composition for an immersion time t2 (min) that satisfies the following inequality:
−0.38 T+173<t2<−1.4 T+720
where T (° C.) is the temperature of the second molten salt composition.

### Claim 30

A manufacturing method for a chemically strengthened glass, the method comprising:
a first step of immersing a lithium-containing glass in a first molten salt composition; and
a second step of immersing the lithium-containing glass in a second molten salt composition that is different in composition from the first molten salt composition, wherein:
an ion exchange for giving a stress that is larger than a CT limit to the lithium-containing glass is performed in the first step; and
a step of reducing the stress to a value lower than the CT limit is executed in the second step.

### Claim 31 (depends on 30)

The manufacturing method for a chemically strengthened glass according to claim 30, wherein:
the first molten salt composition contains lithium ions; and
the second molten salt composition contains potassium ions and lithium ions.

### Claim 32

A chemically strengthened glass, wherein:
a base composition comprises, as represented by mol % based on oxides,
SiO2 of 40% to 75%;
Al2O3 of 1% to 20%; and
Li2O of 5% to 35%; and
wherein a stress value CS90 at a depth 90 (μm) from a glass surface satisfies the following inequality:
CS90/{CT2×(t−2×DOL/1,000)}/t≥2.00