# US 2022/0281766 A1 · Glass, method for producing a glass, and glass melting apparatus

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0281766 A1
- Document ID: US20220281766A1
- Status: Published application
- Kind: A1
- Application number: 17/749,478
- Filed: 2022-05-20
- Published: 2022-09-08
- Earliest claimed: 2019-11-21
- Assignees: Schott AG
- Applicants: Schott AG
- Inventors: Armin VOGEL; Joerg HESSENKEMPER; Knut JAKOBI; Klaus-Dieter DUCH; Andreas SPRENGER; Michael HAHN; Klaus-Peter KOENIG; Thomas PFEIFFER
- Web page: https://patentgrep.com/patent/US20220281766A1

## CPC

- C03C 3/089: containing boron
- C03B 5/03: Tank furnaces
- C03B 5/1672: {Use of materials therefor}
- C03B 5/225: Refining (C03B5/18 takes precedence {; Refining agents C03C1/004})
- C03B 5/43: Use of materials for furnace walls, e.g. fire-bricks
- C03C 3/078: containing an oxide of a divalent metal, e.g. an oxide of zinc
- C03C 3/083: containing aluminium oxide or an iron compound
- C03C 3/087: containing calcium oxide, e.g. common sheet or container glass
- C03C 3/091: containing aluminium
- C03C 3/093: containing zinc or zirconium
- C03B 5/027: by passing an electric current between electrodes immersed in the glass bath, i.e. by direct resistance heating
- C03C 2201/10: containing boron (C03C2201/14 takes precedence)
- C03C 2201/32: containing aluminium (C03C2201/36 takes precedence)
- C03C 2201/50: containing alkali metals
- C03C 2201/54: containing beryllium, magnesium or alkaline earth metals
- C03C 2203/10: Melting processes
- G01N 21/59: Transmissivity (G01N21/25 takes precedence)
- G01N 33/386: {Glass}
- C03C: CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
- C03B: MANUFACTURE, SHAPING, OR SUPPLEMENTARY PROCESSES
- G01N: INVESTIGATING OR ANALYSING MATERIALS BY DETERMINING THEIR CHEMICAL OR PHYSICAL PROPERTIES (measuring or testing apparatus or processes other than immunoassay, involving enzymes or microorganisms C12M, C12Q)

## Abstract

A glass element has, per kg of glass, 50 or fewer inclusions having a size of 2 μm to 10 μm. The glass element can be made of borosilicate glass.

## Claims

### Claim 1

A glass element made of borosilicate glass, wherein the glass element has, per kg of glass, 50 inclusions or fewer having a size from 2 μm to 10 μm.

### Claim 2 (depends on 1)

The glass element according to claim 1, wherein the glass element has, per kg of glass, 2000 inclusions or fewer having a size of 10 μm or less.

### Claim 3 (depends on 1)

The glass element according to claim 1, wherein the glass element has, per kg of glass, 50 inclusions or fewer having a size 50 μm or less, and/or a size of 50 nm or more.

### Claim 4 (depends on 1)

The glass element according to claim 1, wherein the glass element has, per kg of glass, 40 inclusions or fewer.

### Claim 5 (depends on 1)

The glass element according to claim 1, wherein the inclusions comprise metallic inclusions, and wherein the glass element has, per kg of glass, 40 metallic inclusions or fewer having a size of 50 μm or less.

### Claim 6 (depends on 1)

The glass element according to claim 1, wherein the inclusions comprise nonmetallic inclusions, and wherein the glass element has, per kg of glass 25 nonmetallic inclusions or fewer having a size of 2 μm to 50 μm.

### Claim 7 (depends on 1)

The glass element according to claim 1, wherein the inclusions comprise bubbles, wherein the glass element has, per kg of glass, 25 bubbles or fewer having a size of 50 μm or less, and/or 50 nm or more.

### Claim 8 (depends on 1)

The glass element according to claim 1, wherein the glass element has a composition that comprises, in wt %:
SiO2 60 to 90%, preferably 76% to 90%;
B2O3 0 to 20%;
Al2O3 0 to 20%;
Li2O 0 to 10%;
Na2O 0 to 10%;
K2O 0 to 10 %;
MgO 0 to 10 %;
CaO 0 to 10 %;
SrO 0 to 10 %; and
BaO 0 to 10%.

### Claim 9 (depends on 1)

The glass element according to claim 1, wherein the glass element has at least one feature selected from the group consisting of:
i) a weight of the glass element is 0.01 kg to 350 kg;
ii) a glass plate form with a thickness from 0.01 cm to 10 cm;
iii) a glass plate form with a length and width from 1 cm to 500 cm;
iv) a transmission of the glass element, normalized to a glass element in the form of a glass plate with a thickness of 6.5 mm at a wavelength of 400 nm to 800 nm, that is 70% or more; and
v) no inclusions having a size greater than 50 μm.

### Claim 10 (depends on 1)

The glass element according to claim 1, wherein the glass element is a glass plate or a glass tube.

### Claim 11 (depends on 1)

The glass element according to claim 1, wherein the glass element has, per kg of glass, 2000 inclusions or fewer having a size of 50 nm to 500 nm.

### Claim 12 (depends on 1)

The glass element according to claim 1, wherein the glass element has, per kg of glass, 2000 inclusions or fewer having a size of 500 nm to 2 μm.

### Claim 13

A method for producing a glass element made of borosilicate glass comprising the steps:
i) providing a batch, comprising, in wt %:
SiO2 60 to 90%, preferably 76% to 90%;
B2O3 0 to 20%;
Al2O3 0 to 20%;
Li2O 0 to 10%;
Na2O 0 to 10%;
K2O 0 to 10%;
MgO 0 to 10 %;
CaO 0 to 10 %;
SrO 0 to 10 %; and
BaO 0 to 10 %;
ii) heating the batch to form a glass melt,
iii) conditioning the glass melt, and
iv) cooling the glass melt to provide the glass element,
wherein, during step ii) and/or iii):
a) the glass melt is heated at least in part with an electric resistance heater by subjecting electrodes to a heating current, wherein, as heating current, an alternating current with a frequency from 1 kHz and 200 kHz is used;
b) a contact surface with which the glass melt is in contact comprises 30% or more contact material in the form of melt-cast zirconium oxide material with a proportion of over 70 wt % ZrO2; and
c) from 1% to 50% of a volumetric flow is withdrawn from a bottom material of the glass melt in a bottom region of the glass melt.

### Claim 14 (depends on 13)

The method according to claim 13, further comprising during step ii) and/or iii), a viscosity of the glass melt is brought to and/or maintained at from 30 Pas and 450 Pas.

### Claim 15 (depends on 13)

The method according to claim 13, wherein the alternating current has a frequency from 1 kHz to 100 kHz.

### Claim 16 (depends on 13)

The method according to claim 13, further comprising a contact surface with which the glass melt is in contact comprises 60% or more contact material in the form of melt-cast zirconium oxide material with a proportion of 75 wt % or more ZrO2.

### Claim 17 (depends on 13)

The method according to claim 13, wherein5% to 40% of a volumetric flow is withdrawn from a bottom material of the glass melt in a bottom region of the glass melt.

### Claim 18

A glass melting apparatus comprising:
a first heating device for heating a batch to form a glass melt,
a conditioning device for conditioning the glass melt, and
a bottom withdrawal device for withdrawing bottom material of the glass melt,
wherein the first heating device and/or the conditioning device comprises a second heating device that has at least two electrodes for resistance heating; and
wherein
A) the second heating device is configured so that the at least two electrodes are subjected to a heating current in the form of an alternating current with a frequency from 1 kHz to 200 kHz; and/or
B) a contact surface with which the glass melt is in contact comprises 30% or more contact material in the form of melt-cast zirconium oxide material with a proportion of over 70 wt % ZrO2; and/or
C) the bottom withdrawal device is configured to withdraw from 1% to 50% of a volumetric flow from the bottom material of the glass melt in a bottom region of the first heating device and/or the conditioning device.

### Claim 19

A method for operating a glass melting apparatus that comprises a first heating device for heating a batch to form a glass melt, a conditioning device for conditioning the glass melt, and a bottom withdrawal device for withdrawing bottom material of the glass melt, wherein the first heating device and/or the conditioning device comprises a second heating device that has at least two electrodes for resistance heating, the method comprising:
I) operating the second heating device by subjecting the electrodes to a heating current that is an alternating current with a frequency from 1 kHz to 200 kHz,
II) bringing the glass melt into contact with a contact surface that comprises 30% or more melt-cast zirconium oxide material with a proportion of over 70 wt % ZrO2; and
III) operating the bottom withdrawal device so that from 1% to 50% of the volumetric flow is withdrawn from a bottom material of the glass melt in a bottom region of the glass melt.