# US 2022/0281040 A1 · Aluminum alloy brazing sheet and manufacturing method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0281040 A1
- Document ID: US20220281040A1
- Status: Published application
- Kind: A1
- Application number: 17/628,370
- Filed: 2020-07-06
- Published: 2022-09-08
- Earliest claimed: 2019-07-26
- Assignees: Uacj Corporation
- Applicants: UACJ Corporation
- Inventors: Tomoki Yamayoshi; Hidetoshi Kumagai; Hirokazu Tanaka; Taketoshi Toyama; Naoki Sugimoto; Nobuhiro Honma; Shogo Yamada; Takahiro Shinoda
- Web page: https://patentgrep.com/patent/US20220281040A1

## CPC

- B23K 35/286: {Al as the principal constituent}
- B23K 35/0238: {layered}
- B23K 35/22: characterised by the composition or nature of the material
- B23K 35/28: with the principal constituent melting at less than 950°C
- B23K 35/40: Making wire or rods for soldering or welding
- B32B 15/016: {all layers being formed of aluminium or aluminium alloys}
- B32B 15/20: comprising aluminium or copper {(B32B15/016 and B32B15/017 take precedence)}
- C22C 21/00: Alloys based on aluminium
- C22C 21/02: with silicon as the next major constituent
- C22C 21/08: with silicon
- C22F 1/04: of aluminium or alloys based thereon
- C22F 1/043: of alloys with silicon as the next major constituent
- C22F 1/047: of alloys with magnesium as the next major constituent
- C22F 1/00: Changing the physical structure of non-ferrous metals or alloys by heat treatment or by hot or cold working (apparatus for mechanical working of metal B21, B23, B24)
- B23K: SOLDERING OR UNSOLDERING; WELDING; CLADDING OR PLATING BY SOLDERING OR WELDING; CUTTING BY APPLYING HEAT LOCALLY, e.g. FLAME CUTTING; WORKING BY LASER BEAM
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)

## Abstract

An aluminum alloy brazing sheet is formed of a four-layer material formed of a brazing material, an intermediate material, a core material, and a. brazing material. The intermediate material comprises Mg of 0.40 to 6.00 mass %, and has a total of contents of Mn, Cr, and Zr being 0.10 mass % or more. The core material comprises Mg of 0.20 to 2.00 mass % and comprises one or two or more of Mn of 1.80 mass % or less, Si of 1.05 mass % or less, Fe of 1.00 mass % or less, Cu of 1.20 mass % or less, Ti of 0.30 mass % or less, Zr of 0.30 mass % or less, and Cr of 0.30 mass % or less. Each of the core material and the intermediate material has a grain size of 20 to 300 μm.

## Claims

### Claim at position 1

1-48. (canceled)

### Claim 49

An aluminum alloy brazing sheet used for brazing of an aluminum material in an inert gas atmosphere or in vacuum and
formed of a four-layer material in which a brazing material, an intermediate material, a core material, and a brazing material are stacked in this order,
the intermediate material being formed of an aluminum alloy and having a grain size of 20 to 300 μm, the aluminum alloy comprising Mg of 0.40 to 6.00 mass %, and optionally one or two or more of Zn of 8.00 mass % or less, Si of 13.00 mass % or less, Bi of 1.00 mass % or less, In of 0.100 mass % or less, Sn of 0.100 mass % or less, and Fe of 1.00 mass % or less, with the balance being aluminum and inevitable impurities,
the core material being formed of an aluminum alloy and having a grain size of 20 to 300 μm, the aluminum alloy comprising Mg of 0.20 to 2.00 mass % and further comprising one or two or more of Mn of 1.80 mass % or less, Si of 1.50 mass % or less, Fe of 1.00 mass % or less, Cu of 1.20 mass % or less, Ti of 0.30 mass % or less, Zr of 0.30 mass % or less, and Cr of 0.30 mass % or less, with the balance being aluminum and inevitable impurities,
each of the brazing materials being formed of an aluminum alloy comprising Si of 4.00 to 13.00 mass % and further comprising one or two or more of Mn of 2.00 mass % or less, Ti of 0.30 mass % or less, Zr of 0.30 mass % or less, and Cr of 0.30 mass % or less, and optionally one or two or more of Bi of 1.00 mass % or less, Na of 0.050 mass % or less, Sr of 0.050 mass % or less, Sb of 0.050 mass % or less, Mg of 2.00 mass % or less, Zn of 8.00 mass % or less, In of 0.100 mass % or less, Sn of 0.100 mass % or less, Cu of 4.00 mass % or less, and Fe of 1.00 mass % or less, with the balance being, aluminum and inevitable impurities, and
in a drop-type fluidity test, a ratio α (α=Ka/Kb) of a fluid coefficient Ka after a 5% strain is applied to a fluid coefficient Kb before the strain is applied being 0.55 or more.

### Claim 50 (depends on 49)

The aluminum alloy brazing sheet according to claim 49, wherein the intermediate material further comprises one or two or more of Mn of 2.00 mass % or less, Cu of 1.20 mass % or less, Cr of 0.30 mass % or less, and Zr of 0.30 mass % or less, and a total of contents of Mn, Cr, and Zr is 0.1 mass % or more.

### Claim 51

An aluminum alloy brazing sheet used for brazing of an aluminum material in an inert gas atmosphere or in vacuum and
formed of a five-layer material in which a brazing material, an intermediate material, a core material, an intermediate material, and a brazing material are stacked in this order,
each of the intermediate materials being formed of an aluminum alloy and having a grain size of 2.0 to 300 μm, the aluminum alloy comprising Mg of 0.40 to 6.00 mass %, and optionally one or two or more of Zn of 8.00 mass % or less, Si of 13.00 mass % or less, Bi of 1.00 mass % or less, In of 0.100 mass % or less, Sn of 0.100 mass % or less, and Fe of 1.00 mass % or less, with the balance being aluminum and inevitable impurities,
the core material being formed of an aluminum alloy and having a grain size of 20 to 300 μm, the aluminum alloy comprising Mg of 0.20 to 2.00 mass % and further comprising one or two or more of Mn of 1.80 mass % or less, Si of 1.50 mass % or less, Fe of 1.00 mass % or less, Cu of 1.20 mass % or less, Ti of 0.30 mass % or less, Zr of 0.30 mass % or less, and Cr of 0.30 mass % or less, with the balance being aluminum and inevitable impurities,
each of the brazing materials being formed of an aluminum alloy comprising Si of 4.00 to 13.00 mass % and further comprising one or two or more of Mn of 2.00 mass % or less, Ti of 0.30 mass % or less, Zr of 0.30 mass % or less, and Cr of 0.30 mass % or less, and optionally one or two or more of Bi of 1.00 mass % or less, Na of 0.050 mass % or less, Sr of 0.050 mass % or less, Sb of 0.050 mass % or less, Mg of 2.00 mass % or less, Zn of 8.00 mass % or less, In of 0.100 mass % or less, Sn of 0.100 mass % or less, Cu of 4.00 mass % or less, and Fe of 1.00 mass % or less, with the balance being aluminum and inevitable impurities, and
in a drop-type fluidity test, a ratio α (α=Ka/Kb) of a fluid coefficient Ka after a 5% strain is applied to a fluid coefficient Kb before the strain is applied being 0.55 or more.

### Claim 52 (depends on 51)

The aluminum alloy brazing sheet according to claim 51, wherein each of the intermediate materials further comprises one or two or more of Mn of 2.00 mass % or less, Cu of 1.20 mass % or less, Cr of 0.30 mass % or less, and Zr of 0.30 mass % or less, and a total of contents of Mn, Cr, and Zr is 0.1 mass % or more.

### Claim 53 (depends on 49)

A method for manufacturing the aluminum alloy brazing sheet according to claim 49, the method comprising executing at least hot working, cold working, one or more intermediate annealings between rolling passes in the cold working, and final annealing after a last pass of the cold working on a stacked structure acquired by stacking a brazing material ingot, an intermediate material ingot, a core material ingot, and a brazing material ingot in this order to acquire the aluminum alloy brazing sheet, wherein
the intermediate material ingot is formed of an aluminum alloy comprising Mg of 0.40 to 6.00 mass %, and optionally one or two or more of Zn of 8.00 mass % or less, Si of 13.00 mass % or less. Bi of 1.00 mass % or less, In of 0.100 mass % or less, Sn of 0.100 mass % or less, and Fe of 1.00 mass % or less, with the balance being aluminum and inevitable impurities,
the core material ingot is formed of an aluminum alloy comprising Mg of 0.20 to 2.00 mass % and further comprising one or two or more of Mn of 1.80 mass % or less, Si of 1.50 mass % or less, Fe of 1.00 mass % or less, Cu of 1.20 mass % or less, Ti of 0.30 mass % or less, Zr of 0.30 mass % or less, and Cr of 0.30 mass % or less, with the balance being aluminum and inevitable impurities,
each of the brazing material ingots is formed of an aluminum alloy comprising Si of 4.00 to 13.00 mass %, and optionally one or two or more of Bi of 1.00 mass % or less, Na of 0.050 mass % or less, Sr of 0.050 mass % or less, Sb of 0.050 mass % or less. Mg of 2.00 mass % or less, Zn of 8.00 mass % or less, In of 0.100 mass % or less, Sn of 0.100 mass % or less, Cu of 4.00 mass % or less, and Fe of 1.00 mass % or less, with the balance being aluminum and inevitable impurities, and
a working ratio (working ratio=((ta−tb)ta)×100) of a thickness tb before the final annealing to a thickness ta after last intermediate annealing among the intermediate annealings is 20 to 70%.

### Claim 54 (depends on 50)

A method for manufacturing the aluminum alloy brazing sheet according to claim 50, the method comprising executing at least hot working, cold working, one or more intermediate annealings between rolling passes in the cold working, and final annealing after a last pass of the cold working on a stacked structure acquired by stacking a brazing material ingot, an intermediate material ingot, a core material ingot, and a brazing material ingot in this order to acquire the aluminum alloy brazing sheet, wherein
the intermediate material ingot is formed of an aluminum alloy comprising Mg of 0.40 to 6.00 mass %, and optionally one or two or more of Zn of 8.00 mass % or less, Si of 13.00 mass % or less, Bi of 1.00 mass % or less, In of 0.100 mass % or less, Sn of 0.100 mass % or less, and Fe of 1.00 mass % or less, with the balance being aluminum and inevitable impurities,
the core material ingot is formed of an aluminum alloy comprising Mg of 0.20 to 2.00 mass % and further comprising one or two or more of Mn of 1.80 mass % or less, Si of 1.50 mass % or less, Fe of 1.00 mass % or less, Cu of 1.20 mass % or less, Ti of 0.30 mass % or less, Zr of 0.30 mass % or less, and Cr of 0.30 mass % or less. with the balance being aluminum and inevitable impurities,
each of the brazing material ingots is formed of an aluminum alloy comprising Si of 4.00 to 13.00 mass %,and optionally one or two or more of Bi of 1.00 mass % or less, Na of 0.050 mass % or less, Sr of 0.050 mass % or less, Sb of 0.050 mass % or less, Mg of 2.00 mass % or less, Zn of 8.00 mass % or less, In of 0.100 mass % or less, Sn of 0.100 mass % or less, Cu of 4.00 mass % or less, and Fe of 1.00 mass % or less, with the balance being aluminum and inevitable impurities, and
a working ratio (working ratio=((ta−tb)/ta)×100) of a thickness tb before the final annealing to a thickness ta after last intermediate annealing among the intermediate annealings is 20 to 70%.

### Claim 55 (depends on 53)

The method for manufacturing the aluminum alloy brazing sheet according to claim 53, wherein the intermediate material ingot further comprises one or two or more of Mn of 2.00 mass % or less, Cu of 1.20 mass % or less, Cr of 0.30 mass % or less, and Zr of 0.30 mass % or less, and a total of contents of Mn, Cr, and Zr is 0.1 mass % or more.

### Claim 56 (depends on 51)

A method for manufacturing the aluminum alloy brazing sheet according to claim 51, the method comprising executing at least hot working, cold working, one or more intermediate annealings between rolling passes in the cold working, and final annealing after a last pass of the cold working on a stacked structure acquired by stacking a brazing material ingot, an intermediate material ingot, a core material ingot, an intermediate material ingot, and a brazing material ingot in this order to acquire the aluminum alloy brazing sheet, wherein
each of the intermediate material ingots is formed of an aluminum alloy comprising Mg of 0.40 to 6.00 mass %, and optionally one or two or more of Zn of 8.00 mass % or less, Si of 13.00 mass % or less. Bi of 1.00 mass % or less, In of 0.100 mass % or less, Sn of 0.100 mass % or less, and Fe of 1.00 mass % or less, with the balance being aluminum and inevitable impurities,
the core material ingot is formed of an aluminum alloy comprising Mg of 0.20 to 2.00 mass % and further comprising one or two or more of Mn of 1.80 mass % or less, Si of 1.50 mass % or less. Fe of 1.00 mass % or less, Cu of 1.20 mass % or less, Ti of 0.30 mass % or less, Zr of 0.30 mass % or less, and Cr of 0,30 mass less, with the balance being aluminum and inevitable impurities,
each of the brazing material ingots is formed of an aluminum alloy comprising Si of 4.00 to 13.00 mass % and further comprising one or two or more of Mn of 2.00 mass % or less, Ti of 0.30 mass % or less, Zr of 0.30 mass % or less, and Cr of 0.30 mass % or less, and optionally one or two or more of Bi of 1.00 mass % or less, Na of 0.050 mass % or less, Sr of 0.050 mass % of less, Sb of 0.050 mass % or less, Mg of 2.00 mass % or less, Zn of 8.00 mass % or less, In of 0.100 mass % or less, Sn of 0.100 mass % or less, Cu of 4.00 mass % or less, and Fe of 1.00 mass % or less, with the balance being aluminum and inevitable impurities, and
a working ratio (working ratio=((ta−tb)/ta)×100) of a thickness tb before the final annealing to a thickness ta after last intermediate annealing among the intermediate annealings is 20 to 70%.

### Claim 57 (depends on 52)

A method for manufacturing the aluminum alloy brazing sheet according to claim 52, the method comprising executing at least hot working, cold working, one or more intermediate annealings between rolling passes in the cold working, and final annealing after a last pass of the cold working on a stacked structure acquired by stacking a brazing material ingot, an intermediate material ingot, a core material ingot, an intermediate material ingot, and a brazing material ingot in this order to acquire the aluminum alloy brazing sheet, wherein
each of the intermediate material ingots is formed of an aluminum alloy comprising Mg of 0.40 to 6.00 mass %, and optionally one or two or more of Zn of 8.00 mass % or less, Si of 13.00 mass % or less, Bi of 1.00 mass % or less, In of 0.100 mass % or less, Sn of 0.100 mass % or less, and Fe of 1.00 mass % or less, with the balance being aluminum and inevitable impurities, the core material ingot is formed of an aluminum alloy comprising Mg of 0.20 to 2.00 mass % and further comprising one or two or more of Mn of 1.80 mass % or less, Si of 1.50 mass % or less, Fe of 1.00 mass % or less, Cu of 1.20 mass % or less, Ti of 0.30 mass % or less, Zr of 0.30 mass % or less, and Cr of 0.30 mass % or less, with the balance being aluminum and inevitable impurities,
each of the brazing material ingots is formed of an aluminum alloy comprising Si of 4.00 to 13.00 mass % and further comprising one or two or more of Mn of 2.00 mass % or less, Ti of 0.30 mass % or less, Zr of 0.30 mass % or less, and Cr of 0.30 mass % or less, and optionally one or two or more of Bi of 1.00 mass % or less, Na of 0.050 mass % or less, Sr of 0.050 mass % or less, Sb of 0.050 mass % or less, Mg of 2.00 mass % or less, Zn of 8.00 mass % or less, In of 0.100 mass % or less, Sn of 0.100 mass % or less, Cu of 4.00 mass % or less, and Fe of 1.00 mass % or less, with the balance being aluminum and inevitable impurities, and
a working ratio (working ratio=(ta−tb)ta)×100) of a thickness tb before the final annealing to a thickness ta after last intermediate annealing among the intermediate annealings is 20 to 70%.

### Claim 58 (depends on 56)

The method for manufacturing the aluminum alloy brazing sheet according to claim 56, wherein each of the intermediate material ingots further comprises one or two or more of Mn of 2.00 mass % or less, Cu of 1.20 mass % or less, Cr of 0.30 mass % or less, and Zr of 0.30 mass % or less, and a total of contents of Mn, Cr, and Zr is 0.1 mass % or more.