# US 2022/0278355 A1 · Method of preparation of a garnet-type inorganic material

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0278355 A1
- Document ID: US20220278355A1
- Status: Published application
- Kind: A1
- Application number: 17/625,996
- Filed: 2020-07-29
- Published: 2022-09-01
- Earliest claimed: 2019-08-06
- Assignees: Rhodia Operations
- Applicants: Rhodia Operations
- Inventors: Réka TOTH; Laure BERTRY; Valérie BUISSETTE; Thierry LE MERCIER; Marc-David BRAIDA; Robin AMISSE
- Web page: https://patentgrep.com/patent/US20220278355A1

## CPC

- H01M 10/056: characterised by the materials used as electrolytes, e.g. mixed inorganic/organic electrolytes
- H01M 10/0562: Solid materials
- C01G 25/006: {Compounds containing zirconium, with or without oxygen or hydrogen, and containing two or more other elements}
- C01G 33/006: {Compounds containing niobium, with or without oxygen or hydrogen, and containing two or more other elements}
- C01G 49/0054: {containing one rare earth metal, yttrium or scandium}
- C04B 35/486: Fine ceramics
- C04B 35/62675: {characterised by the treatment temperature}
- C04B 35/62685: {characterised by the order of addition of constituents or additives}
- C04B 35/632: Organic additives
- C04B 35/63488: {Polyethers, e.g. alkylphenol polyglycolether, polyethylene glycol [PEG], polyethylene oxide [PEO]}
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- C01P 2002/30: Three-dimensional structures
- C01P 2002/52: containing elements as dopants
- C01P 2002/54: one element only
- C01P 2004/51: Particles with a specific particle size distribution
- C01P 2004/61: Micrometer sized, i.e. from 1-100 micrometer
- C01P 2004/62: Submicrometer sized, i.e. from 0.1-1 micrometer
- C01P 2006/40: Electric properties
- C04B 2235/3203: Lithium oxide or oxide-forming salts thereof
- C04B 2235/3217: Aluminum oxide or oxide forming salts thereof, e.g. bauxite, alpha-alumina
- C04B 2235/3227: Lanthanum oxide or oxide-forming salts thereof
- C04B 2235/3244: Zirconium oxides, zirconates, hafnium oxides, hafnates, or oxide-forming salts thereof
- C04B 2235/3251: Niobium oxides, niobates, tantalum oxides, tantalates, or oxide-forming salts thereof
- C04B 2235/3258: Tungsten oxides, tungstates, or oxide-forming salts thereof
- C04B 2235/3272: Iron oxides or oxide forming salts thereof, e.g. hematite, magnetite
- C04B 2235/3286: Gallium oxides, gallates, indium oxides, indates, thallium oxides, thallates or oxide forming salts thereof, e.g. zinc gallate
- C04B 2235/443: Nitrates or nitrites
- C04B 2235/444: Halide containing anions, e.g. bromide, iodate, chlorite
- C04B 2235/445: Fluoride containing anions, e.g. fluosilicate
- C04B 2235/5436: micrometer sized, i.e. from 1 to 100 micron
- C04B 2235/5445: submicron sized, i.e. from 0,1 to 1 micron
- C04B 2235/5463: Particle size distributions
- C04B 2235/764: Garnet structure A3B2(CO4)3
- H01M 2300/0077: based on zirconium oxide
- H01M 2300/0091: in the form of mixtures
- Y02E 60/10: Energy storage using batteries
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01G: COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts or peroxyacids C01B15/00; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium, or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds containing nitrogen, other non-metals and metal C01B21/082}; metal amides C01B21/092; nitrites C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; compounds having molecular sieve properties but not having base-exchange properties C01B37/00; compounds having molecular sieve and base-exchange properties, e.g. crystalline zeolites, C01B39/00; cyanides C01C3/08; salts of cyanamide C01C3/16; thiocyanates C01C3/20)
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

The present invention relates to a method of preparation of a garnet-type inorganic material. It also relates to the garnet-type inorganic material itself. The process comprises the following steps: (1) bringing an aqueous solution S comprising (i) a salt of zirconium, (ii) a salt of lanthanum and (iii) a salt of the element A or a precursor of an oxide of element A into contact with an aqueous solution of a basic compound, as a result of which a precipitate suspended in the reaction medium is obtained; (2) stirring the reaction medium obtained at the end of step (1) for at least 30 min; (3) bringing the precipitate obtained at the end of step (2) into contact with an additive selected in the group consisting of: anionic surfactants; nonionic surfactants; polyethylene glycols; carboxylic acids and their salts; and surfactants of the carboxymethylated fatty alcohol ethoxylate type; (4) calcining in air the precipitate recovered at the end of the previous step at a temperature which is at least 400° C.; (5) bringing into contact the product obtained at the end of step (4) with a salt of lithium; (6) calcining in air the product obtained at the end of step (5) at a temperature between 700° C. and 1100° C.; 20 the inorganic compound M comprising or consisting essentially of a garnet oxide or garnet-type oxide containing, as constituent elements, the elements Li, La, Zr and at least one element A selected in the group consisting of Al, Ga, Nb, Fe, W, Ta, or a mixture thereof.

## Claims

### Claim at position 1

1-35. (canceled)

### Claim 36

An inorganic material M comprising a garnet oxide or garnet-type oxide containing, as constituent elements, the elements Li, La, Zr and at least one element A selected from the group consisting of Al, Ga, Nb, Fe, W, Ta, and a mixture thereof, the oxide being described by formula (I):
[Lix1La3ZrzAwO12] (I)
wherein:
x1, z and w are positive real numbers;
1.20<z≤2.10;
0<w≤0.80; and
x1 is derived from the electroneutrality of the oxide; and
exhibiting:
a ratio R50 higher than 50%, R50 being defined by:
R50(%)=(D50−DUS50)/D50×100
wherein D50 and DUS50 are the median diameters of distributions in volume of the diameters of a dispersion of the particles of the inorganic material M in N-methyl-2-pyrrolidone (NMP), obtained with a laser diffractometer, DUS50 being measured after a treatment under ultrasound which consists of inserting an ultrasonic probe into a dispersion of 100 mg of the inorganic material M in 160 mL of NMP and in submitting the dispersion to sonication under a power of 140±10 W for 22 minutes.
and/or
a ratio R90 higher than 50%, R90 being defined by:
R90(%)=(D90−DUS90)/D90×100
wherein D90 and DUS90 correspond to the diameters of the particles for which 90% of the particles have a diameter which is less than D90 and are determined from distributions in volume of the diameters of a dispersion of the particles of the inorganic material M in N-methyl-2-pyrrolidone (NMP), obtained with a laser diffractometer, DUS90 being measured after a treatment under ultrasound which consists of inserting an ultrasonic probe into a dispersion of 100 mg of the inorganic material M in 160 mL of NMP and in submitting the dispersion to sonication under a power of 140±10 W for 22 minutes.

### Claim 37

An inorganic material M comprising a garnet oxide or garnet-type oxide containing, as constituent elements, the elements Li, La, Zr and at least one element A selected from the group consisting of Al, Ga, Nb, Fe, W, Ta, and a mixture thereof, the oxide being described by formula (I):
[Lix1La3ZrzAwO12] (I)
wherein:
x1, z and w are positive real numbers;
1.20<z≤2.10;
0<w≤0.80;
x1 is derived from the electroneutrality of the oxide; and
exhibiting:
a ratio R50 higher than 50%, R50 being defined by:
R50(%)=(D50−Dus50)/D50×100
wherein D50 and DUS50 are the median diameters of distributions in volume of the diameters of a dispersion of the particles of the inorganic material M in N-methyl-2-pyrrolidone (NMP), obtained with a laser diffractometer, DUS50 being measured after a treatment under ultrasound which consists of inserting an ultrasonic probe into a dispersion of 100 mg of the inorganic material M in 160 mL of NMP and in submitting the dispersion to sonication under a power of 140±10 W for 22 minutes.

### Claim 38 (depends on 36)

The inorganic material M according to claim 36 wherein the relative composition of the cations in the inorganic material M corresponds to formula:
Lix1La3ZrzAw (II)
wherein:
w, x and z are positive real numbers;
1.20<z≤2.10;
0<w≤0.80; and
4.00≤x≤10.5.

### Claim 39 (depends on 36)

The inorganic material M according to claim 36 wherein the relative composition of the cations in the inorganic material M corresponds to formula:
LixLa3ZrzA1w1A2w2 (IIa)
wherein:
A1 is selected from the group consisting of Al, Ga, Fe or a combination thereof;
A2 is selected from the group consisting of Nb, Ta or a combination thereof;
w1, w2, x and z are positive real numbers;
1.20<z≤2.10;
0<w1≤0.20;
0.10<w2≤0.80;
w1 and w2 being such that w=w1+w2 and w≤0.80; and
5.60≤x≤10.35.

### Claim 40 (depends on 36)

The inorganic material M according to claim 36 wherein the relative composition of the cations in the inorganic material M corresponds to formula:
LixLa3ZrzA1w1A2w2 (IIb)
wherein:
A1 is selected from the group consisting of Al, Ga, Fe or a combination thereof;
A2 is W;
w1, w2, x and z are positive real numbers;
1.20<z≤2.10;
0<w1≤0.20;
0.10<w2≤0.80;
w1 and w2 being such that w=w1+w2 and w≤0.80; and
4.80≤x≤10.20.

### Claim 41 (depends on 36)

The inorganic material M according to claim 36 wherein Zr is partly replaced by Hf in the oxide.

### Claim 42 (depends on 36)

The inorganic material M according to claim 36 wherein the primary particles of the inorganic material M exhibit a d50 between 0.5 μm and 7.0 μm.

### Claim 43 (depends on 36)

The inorganic material M according to claim 36 wherein the particles of the inorganic material M exhibt a D50 between 10.0 and 50.0 μm.

### Claim 44 (depends on 36)

A process of preparation of the inorganic material M of claim 36, the process comprising the following steps:
(1) bringing an aqueous solution S comprising (i) a salt of zirconium, (ii) a salt of lanthanum and (iii) a salt of the element A or a precursor of an oxide of element A into contact with an aqueous solution of a basic compound, as a result of which a precipitate suspended in the reaction medium is obtained;
(2) stirring the reaction medium obtained at the end of step (1) for at least 30 min;
(3) bringing the precipitate obtained at the end of step (2) into contact with an additive selected from the group consisting of: anionic surfactants; nonionic surfactants; polyethylene glycols;
carboxylic acids and their salts; and surfactants of the carboxymethylated fatty alcohol ethoxylate type;
(4) calcining in air the precipitate recovered at the end of the previous step at a temperature which is at least 400° C.;
(5) bringing into contact the product obtained at the end of step (4) with a salt of lithium;
(6) calcining in air the product obtained at the end of step (5) at a temperature between 700° C. and 1100° C.;
the inorganic compound M comprising or consisting essentially of a garnet oxide or garnet-type oxide containing, as constituent elements, the elements Li, La, Zr and at least one element A selected in the group consisting of Al, Ga, Nb, Fe, W, Ta, or a mixture thereof.

### Claim 45 (depends on 44)

The process according to claim 44 wherein the salt of zirconium is selected from the group of zirconium nitrate and zirconium chloride.

### Claim 46 (depends on 44)

The process according to claim 44 wherein in step (2), the reaction medium is stirred for at least 30 minutes and the temperature of the reaction medium is between 50° C. and 200° C.

### Claim 47 (depends on 44)

The process according to claim 44 wherein the additive is a carboxylic acid or a salt thereof.

### Claim 48 (depends on 44)

The process according to claim 44 wherein the temperature of calcination in step (4) is between 400° C. and 800° C.

### Claim 49 (depends on 44)

The process according to claim 44 wherein the bringing into contact of step (5) consists of impregnating the product obtained at the end of the step (4) with an aqueous solution of a salt of lithium or in mixing together the product obtained at the end of step (4) and the salt of lithium, both being in the powder form.

### Claim 50 (depends on 44)

The process according to claim 44 wherein in step (6), the product obtained at the end of step (5) is first calcined in air at a temperature between 700° C. and 900° C. and then calcined in air at a temperature between 900° C. and 1100° C.

### Claim 51 (depends on 44)

An inorganic material M obtainable by the process according to claim 44.

### Claim 52 (depends on 36)

A composition (C) comprising:
(i) the inorganic material M of claim 36;
(ii) at least one electro-active compound (EAC);
(iii) optionally at least one lithium ion-conducting material (LiCM) other than the inorganic material M;
(iv) optionally at least one electro-conductive material (ECM);
(v) optionally a lithium salt (LIS); and
(vi) optionally at least one polymeric binding material (P).

### Claim 53 (depends on 52)

An electrode (E) comprising:
a metal substrate;
directly adhered onto said metal substrate, at least one layer L made of a composition (Cof claim 52.

### Claim 54 (depends on 36)

A separator (SP) comprising:
the inorganic material M claim 36;
optionally at least one polymeric binding material (P);
optionally at least one metal salt, notably a lithium salt; and
optionally at least one plasticizer.

### Claim 55 (depends on 36)

Lithium ion battery comprising the inorganic material M of of claim 36.