# US 2022/0090267 A1 · Grain-oriented electrical steel sheet and method for manufacturing the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0090267 A1
- Document ID: US20220090267A1
- Status: Published application
- Kind: A1
- Application number: 17/421,762
- Filed: 2020-01-16
- Published: 2022-03-24
- Earliest claimed: 2019-01-16
- Assignees: Nippon Steel Corporation
- Applicants: Nippon Steel Corporation
- Inventors: Shinji YAMAMOTO; Yoshiyuki USHIGAMI; Shinsuke TAKATANI; Shuichi NAKAMURA
- Web page: https://patentgrep.com/patent/US20220090267A1

## CPC

- C23C 22/07: containing phosphates
- C21D 1/76: Adjusting the composition of the atmosphere
- C21D 1/84: Controlled slow cooling (cooling-beds for metal rolling B21B43/00)
- C21D 3/04: Decarburising
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/1255: {with diffusion of elements, e.g. decarburising, nitriding}
- C21D 8/1261: {following hot rolling}
- C21D 8/1272: {Final recrystallisation annealing}
- C21D 8/1283: {Application of a separating or insulating coating}
- C21D 9/46: for sheet metals
- C23C 22/33: containing also phosphates
- C23C 22/74: for obtaining burned-in conversion coatings
- H01F 1/18: with insulating coating
- C21D 6/008: {containing Si}
- C21D 8/1288: {Application of a tension-inducing coating}
- C21D 2201/05: Grain orientation
- C22C 38/001: {containing N}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/16: containing copper
- C22C 38/60: containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
- Y02P 10/20: Recycling
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

A grain-oriented electrical steel sheet includes a base steel sheet which contains Si and Mn, an intermediate layer which is disposed on a surface of the base steel sheet and contains a silicon oxide as a main component, and an insulation coating which is disposed on a surface of the intermediate layer. A final-annealed film is not substantially present on a surface of the base steel sheet. In a surface layer region of grain-oriented electrical steel sheet, a Mn-depletion layer having a valley portion of a Mn content in which a Mn content is lower than an average Mn content of the base steel sheet in a region deeper than the surface layer region is provided, and a Mn-rich layer having a peak portion of a Mn content in which a Mn content is higher than that in the valley portion of the Mn content is provided in a region closer to a surface of the insulation coating than the Mn-depletion layer.

## Claims

### Claim 1

A grain-oriented electrical steel sheet, comprising:
a base steel sheet which contains Si and Mn;
an intermediate layer which is disposed on a surface of the base steel sheet and contains a silicon oxide as a main component; and
an insulation coating which is disposed on a surface of the intermediate layer,
wherein a final-annealed film is substantially not present on a surface of the base steel sheet, and
in a surface layer region,
a Mn-depletion layer having a valley portion of a Mn content in which a Mn content is lower than an average Mn content of the base steel sheet in a region deeper than the surface layer region is provided, and
a Mn-rich layer having a peak portion of a Mn content in which a Mn content is higher than that in the valley portion of the Mn content is provided in a region closer to a surface of the insulation coating than the Mn-depletion layer.

### Claim 2 (depends on 1)

The grain-oriented electrical steel sheet according to claim 1, wherein:
in a profile for a depth of a Mn standardized optical emission intensity calculated using the following Equations 1-1 and 1-2 from data of an optical emission intensity and a measurement time of Mn measured by a glow-discharge optical emission analysis for the grain-oriented electrical steel sheet, when a point having a maximum depth among points having a Mn standardized optical emission intensity of 0.9 is defined as a point A,
the surface layer region is a region from the surface of the insulation coating to a depth of the point A,
a point B at which the Mn standardized optical emission intensity is 0.50 or more and is the local maximum is located in the surface layer region,
a point C at which the Mn standardized optical emission intensity is the local minimum is located between the point A and the point B in the surface layer region,
the valley portion of the Mn content is a region having a depth of 0.1 μm before and after the point C,
the peak portion of the Mn content is a region having a depth of 0.1 μm before and after the point B, and
when an intermediate depth between the depth of the point B and the depth of the point C is defined as a boundary depth, and the Mn standardized optical emission intensity at the boundary depth is defined as a boundary Mn standardized optical emission intensity,
the Mn-depletion layer is a region from the boundary depth to the depth of the point A, and
the Mn-rich layer is present on the surface side of the insulation coating from the point B and is a region from a depth of a point having the same Mn standardized optical emission intensity as the boundary Mn standardized optical emission intensity to the boundary depth,
depth of d μm of each of measurement points=measurement depth in unit μm after measurement end/time in unit seconds until measurement end×measurement time in unit seconds of measurement point Equation 1-1,
Mn standardized optical emission intensity at depth of d μm=optical emission intensity of Mn at depth of d μm/average optical emission intensity of Mn at depth of 25 μm to 30 μm Equation 1-2.

### Claim 3 (depends on 2)

The grain-oriented electrical steel sheet according to claim 2, wherein the point B and the point C in the surface layer region satisfy a relationship of the following Equation 2,
Mn standardized optical emission intensity at point B-Mn standardized optical emission intensity at point C≥0.05 Equation 2.

### Claim 4 (depends on 2)

The grain-oriented electrical steel sheet according to claim 2, wherein a distance between the point A and the point B in a depth direction calculated from the following Equation 3 is 0 to 10.0 μm,
distance between point A and point B in depth direction at unit μm=depth in unit μm at point B-depth in unit μm at point A Equation 3.

### Claim 5 (depends on 2)

The grain-oriented electrical steel sheet according to claim 2, wherein:
the insulation coating contains no Si,
in a profile for a depth of a Si standardized optical emission intensity calculated using the following Equations 2-1 and 2-2 from data of an optical emission intensity and a measurement time of Si measured by the glow-discharge optical emission analysis for the grain-oriented electrical steel sheet, the surface layer region has a point D at which the Si standardized optical emission intensity is the local maximum, and
a distance between the point B and the point D in the depth direction calculated from the following Equation 4 is 0 to 1.0 μm,
depth d μm of each of measurement points=measurement depth in unit μm after measurement end/time in unit seconds until measurement end×measurement time in unit seconds of measurement point Equation 2-1,
Si standardized optical emission intensity at depth of d μm=optical emission intensity of Si at depth of d μm/average optical emission intensity of Si at depth of 25 μm to 30 μm Equation 2-2,
distance in unit μm between point B and point D in depth direction=depth in unit μm at point B-depth in unit μm at point D Equation 4.

### Claim 6 (depends on 2)

The grain-oriented electrical steel sheet according to claim 2, wherein:
the insulation coating contains Si,
when, in a profile for a depth of a Si standardized optical emission intensity calculated using the following Equations 2-1 and 2-2 from data of an optical emission intensity and a measurement time of Si measured by the glow-discharge optical emission analysis for the grain-oriented electrical steel sheet, and a profile for a depth of a Si difference quotient calculated using the following Equation 5-1,
in the surface layer region, in a region in which the Si difference quotient is a negative value, a point at which the Si difference quotient is the local minimum and the Si difference quotient is −0.5 or less is defined as a point V, and a point at which the Si difference quotient is the local maximum, is present on the surface side of the insulation coating from the point V, and is closest to the point V is defined as a point Z, and
in a profile for a depth of a Mn difference quotient calculated from the Mn standardized optical emission intensity using the following Equation 5-2,
in the surface layer region, a point at which the Mn difference quotient is maximum is defined as a point Y, and a point at which the Mn difference quotient is minimum is defined as a point X, and
a point which is present in a region from the point X to the point Y and at which the Mn difference quotient is 0 is defined as a point W,
a distance between the point W and the point Z in the depth direction calculated from the following Equation 6 is 0 to 1.0 μm, and
the Mn difference quotient at the point Y and the Mn difference quotient at the point X satisfy a relationship of the following Equation 7,
depth d μm of each of measurement points=measurement depth in unit μm after measurement end/time in unit seconds until measurement end×measurement time in unit seconds of measurement point Equation 2-1,
Si standardized optical emission intensity at depth of d μm=optical emission intensity of Si at depth of d μm/average optical emission intensity of Si at depth of 25 μm to 30 μm Equation 2-2,
Si difference quotient at depth of d μm={Si standardized optical emission intensity at depth of d μm-Si standardized optical emission intensity at depth (d−h) μm}/h μm Equation 5-1,
Mn difference quotient at depth d μm={Mn standardized optical emission intensity at depth of d μm-Mn standardized optical emission intensity at depth (d−h) μm}/h μm Equation 5-2,
distance in unit μm between point W and point Z in the depth direction=depth in unit μm at point W-depth in unit μm at point Z Equation 6,
Mn difference quotient at point Y-Mn difference quotient at point X≥0.015 Equation 7,
wherein, in the above-described Equations 5-1 and 5-2, h indicates a sampling interval of the data in μm in the glow-discharge optical emission analysis.

### Claim 7 (depends on 1)

A method for manufacturing the grain-oriented electrical steel sheet according to claim 1, comprising:
a hot rolling process of heating and then hot-rolling a slab containing Si and Mn and obtaining a hot-rolled steel sheet;
a hot-band annealing process of performing hot-band annealing on the hot-rolled steel sheet and obtaining an annealed steel sheet;
a cold rolling process of cold-rolling the annealed steel sheet once or twice or more with intermediate annealing interposed therebetween and obtaining a cold-rolled steel sheet;
a decarburization annealing process of performing decarburization annealing on the cold-rolled steel sheet and obtaining a decarburization-annealed steel sheet;
a final annealing process of heating the decarburization-annealed steel sheet in a state which an annealing separator having a MgO content of 10 mass % to 50 mass % is applied to the surface of the decarburization-annealed steel sheet, then removing the annealing separator from the surface, and obtaining a final-annealed steel sheet;
an intermediate layer forming process of performing thermal oxidation annealing on the final-annealed steel sheet and forming an intermediate layer on a surface of the final-annealed steel sheet; and
an insulation coating forming process of forming an insulation coating on the intermediate layer,
wherein, in a cooling process of the final annealing process,
when a final annealing temperature is 1100° C. or higher, T1 is set to 1100° C., and when the final annealing temperature is less than 1100° C., T1 is set as the final annealing temperature,
cooling in a temperature range of T1 to 500° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.3 to 100000, and
in a cooling process of the insulation coating forming process,
cooling in a temperature range of 800° C. to 600° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.10 to 0.30 for a residence time of 10 seconds to 60 seconds.

### Claim 8 (depends on 1)

A method for manufacturing the grain-oriented electrical steel sheet according to claim 1, comprising:
a hot rolling process of heating and then hot-rolling a slab containing Si and Mn and obtaining a hot-rolled steel sheet;
a hot-band annealing process of performing hot-band annealing on the hot-rolled steel sheet and obtaining an annealed steel sheet;
a cold rolling process of cold-rolling the annealed steel sheet once or twice or more with intermediate annealing interposed therebetween and obtaining a cold-rolled steel sheet;
a decarburization annealing process of performing decarburization annealing on the cold-rolled steel sheet and obtaining a decarburization-annealed steel sheet;
a final annealing process of heating the decarburization-annealed steel sheet in a state which an annealing separator having a MgO content of 10 mass % to 50 mass % is applied to the surface of the decarburization-annealed steel sheet, then removing the annealing separator on the surface, and obtaining a final-annealed steel sheet; and
an intermediate layer and insulation coating forming process of forming an intermediate layer and an insulation coating on a surface of the final-annealed steel sheet in one process,
wherein, in a cooling process of the final annealing process,
when a final annealing temperature is 1100° C. or higher, T1 is set to 1100° C., and when the final annealing temperature is less than 1100° C., T1 is set as the final annealing temperature,
cooling in a temperature range of T1 to 500° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.3 to 100000,
in the intermediate layer and insulation coating forming process,
an atmosphere in a temperature range of 800° C. to 1150° C. is set to an oxidation degree (PH2O/PH2) of 0.05 to 0.18, and
in a cooling process of the intermediate layer and insulation coating forming process,
cooling in a temperature range of 800° C. to 600° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.10 to 0.30 for a residence time of 10 seconds to 60 seconds.

### Claim 9 (depends on 3)

The grain-oriented electrical steel sheet according to claim 3, wherein a distance between the point A and the point B in a depth direction calculated from the following Equation 3 is 0 to 10.0 μm,
distance between point A and point B in depth direction at unit μm=depth in unit μm at point B-depth in unit μm at point A Equation 3.

### Claim 10 (depends on 3)

The grain-oriented electrical steel sheet according to claim 3, wherein:
the insulation coating contains no Si,
in a profile for a depth of a Si standardized optical emission intensity calculated using the following Equations 2-1 and 2-2 from data of an optical emission intensity and a measurement time of Si measured by the glow-discharge optical emission analysis for the grain-oriented electrical steel sheet, the surface layer region has a point D at which the Si standardized optical emission intensity is the local maximum, and
a distance between the point B and the point D in the depth direction calculated from the following Equation 4 is 0 to 1.0 μm,
depth d μm of each of measurement points=measurement depth in unit μm after measurement end/time in unit seconds until measurement end×measurement time in unit seconds of measurement point Equation 2-1,
Si standardized optical emission intensity at depth of d μm=optical emission intensity of Si at depth of d μm/average optical emission intensity of Si at depth of 25 μm to 30 μm Equation 2-2,
distance in unit μm between point B and point D in depth direction=depth in unit μm at point B-depth in unit μm at point D Equation 4.

### Claim 11 (depends on 4)

The grain-oriented electrical steel sheet according to claim 4, wherein:
the insulation coating contains no Si,
in a profile for a depth of a Si standardized optical emission intensity calculated using the following Equations 2-1 and 2-2 from data of an optical emission intensity and a measurement time of Si measured by the glow-discharge optical emission analysis for the grain-oriented electrical steel sheet, the surface layer region has a point D at which the Si standardized optical emission intensity is the local maximum, and
a distance between the point B and the point D in the depth direction calculated from the following Equation 4 is 0 to 1.0 μm,
depth d μm of each of measurement points=measurement depth in unit μm after measurement end/time in unit seconds until measurement end×measurement time in unit seconds of measurement point Equation 2-1,
Si standardized optical emission intensity at depth of d μm=optical emission intensity of Si at depth of d μm/average optical emission intensity of Si at depth of 25 μm to 30 μm Equation 2-2,
distance in unit μm between point B and point D in depth direction=depth in unit μm at point B-depth in unit μm at point D Equation 4.

### Claim 12 (depends on 3)

The grain-oriented electrical steel sheet according to claim 3, wherein:
the insulation coating contains Si,
when, in a profile for a depth of a Si standardized optical emission intensity calculated using the following Equations 2-1 and 2-2 from data of an optical emission intensity and a measurement time of Si measured by the glow-discharge optical emission analysis for the grain-oriented electrical steel sheet, and a profile for a depth of a Si difference quotient calculated using the following Equation 5-1,
in the surface layer region, in a region in which the Si difference quotient is a negative value, a point at which the Si difference quotient is the local minimum and the Si difference quotient is −0.5 or less is defined as a point V, and a point at which the Si difference quotient is the local maximum, is present on the surface side of the insulation coating from the point V, and is closest to the point V is defined as a point Z, and
in a profile for a depth of a Mn difference quotient calculated from the Mn standardized optical emission intensity using the following Equation 5-2,
in the surface layer region, a point at which the Mn difference quotient is maximum is defined as a point Y, and a point at which the Mn difference quotient is minimum is defined as a point X, and
a point which is present in a region from the point X to the point Y and at which the Mn difference quotient is 0 is defined as a point W,
a distance between the point W and the point Z in the depth direction calculated from the following Equation 6 is 0 to 1.0 μm, and
the Mn difference quotient at the point Y and the Mn difference quotient at the point X satisfy a relationship of the following Equation 7,
depth d μm of each of measurement points=measurement depth in unit μm after measurement end/time in unit seconds until measurement end×measurement time in unit seconds of measurement point Equation 2-1,
Si standardized optical emission intensity at depth of d μm=optical emission intensity of Si at depth of d μm/average optical emission intensity of Si at depth of 25 μm to 30 μm Equation 2-2,
Si difference quotient at depth of d μm={Si standardized optical emission intensity at depth of d μm-Si standardized optical emission intensity at depth (d−h) μm}/h μm Equation 5-1,
Mn difference quotient at depth d μm={Mn standardized optical emission intensity at depth of d μm-Mn standardized optical emission intensity at depth (d−h) μm}/h μm Equation 5-2,
distance in unit μm between point W and point Z in the depth direction=depth in unit μm at point W-depth in unit μm at point Z Equation 6,
Mn difference quotient at point Y-Mn difference quotient at point X≥0.015 Equation 7,
wherein, in the above-described Equations 5-1 and 5-2, h indicates a sampling interval of the data in μm in the glow-discharge optical emission analysis.

### Claim 13 (depends on 4)

The grain-oriented electrical steel sheet according to claim 4, wherein:
the insulation coating contains Si,
when, in a profile for a depth of a Si standardized optical emission intensity calculated using the following Equations 2-1 and 2-2 from data of an optical emission intensity and a measurement time of Si measured by the glow-discharge optical emission analysis for the grain-oriented electrical steel sheet, and a profile for a depth of a Si difference quotient calculated using the following Equation 5-1,
in the surface layer region, in a region in which the Si difference quotient is a negative value, a point at which the Si difference quotient is the local minimum and the Si difference quotient is −0.5 or less is defined as a point V, and a point at which the Si difference quotient is the local maximum, is present on the surface side of the insulation coating from the point V, and is closest to the point V is defined as a point Z, and
in a profile for a depth of a Mn difference quotient calculated from the Mn standardized optical emission intensity using the following Equation 5-2,
in the surface layer region, a point at which the Mn difference quotient is maximum is defined as a point Y, and a point at which the Mn difference quotient is minimum is defined as a point X, and
a point which is present in a region from the point X to the point Y and at which the Mn difference quotient is 0 is defined as a point W,
a distance between the point W and the point Z in the depth direction calculated from the following Equation 6 is 0 to 1.0 μm, and
the Mn difference quotient at the point Y and the Mn difference quotient at the point X satisfy a relationship of the following Equation 7:
depth d μm of each of measurement points=measurement depth in unit μm after measurement end/time in unit seconds until measurement end×measurement time in unit seconds of measurement point Equation 2-1,
Si standardized optical emission intensity at depth of d μm=optical emission intensity of Si at depth of d μm/average optical emission intensity of Si at depth of 25 μm to 30 μm Equation 2-2,
Si difference quotient at depth of d μm={Si standardized optical emission intensity at depth of d μm-Si standardized optical emission intensity at depth (d−h) μm}/h μm Equation 5-1,
Mn difference quotient at depth d μm={Mn standardized optical emission intensity at depth of d μm-Mn standardized optical emission intensity at depth (d−h) μm}/h μm Equation 5-2,
distance in unit μm between point W and point Z in the depth direction=depth in unit μm at point W-depth in unit μm at point Z Equation 6,
Mn difference quotient at point Y-Mn difference quotient at point X≥0.015 Equation 7,
wherein, in the above-described Equations 5-1 and 5-2, h indicates a sampling interval of the data in m in the glow-discharge optical emission analysis.

### Claim 14 (depends on 2)

A method for manufacturing the grain-oriented electrical steel sheet according to claim 2, comprising:
a hot rolling process of heating and then hot-rolling a slab containing Si and Mn and obtaining a hot-rolled steel sheet;
a hot-band annealing process of performing hot-band annealing on the hot-rolled steel sheet and obtaining an annealed steel sheet;
a cold rolling process of cold-rolling the annealed steel sheet once or twice or more with intermediate annealing interposed therebetween and obtaining a cold-rolled steel sheet;
a decarburization annealing process of performing decarburization annealing on the cold-rolled steel sheet and obtaining a decarburization-annealed steel sheet;
a final annealing process of heating the decarburization-annealed steel sheet in a state which an annealing separator having a MgO content of 10 mass % to 50 mass % is applied to the surface of the decarburization-annealed steel sheet, then removing the annealing separator from the surface, and obtaining a final-annealed steel sheet;
an intermediate layer forming process of performing thermal oxidation annealing on the final-annealed steel sheet and forming an intermediate layer on a surface of the final-annealed steel sheet; and
an insulation coating forming process of forming an insulation coating on the intermediate layer,
wherein, in a cooling process of the final annealing process,
when a final annealing temperature is 1100° C. or higher, T1 is set to 1100° C., and when the final annealing temperature is less than 1100° C., T1 is set as the final annealing temperature,
cooling in a temperature range of T1 to 500° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.3 to 100000, and
in a cooling process of the insulation coating forming process,
cooling in a temperature range of 800° C. to 600° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.10 to 0.30 for a residence time of 10 seconds to 60 seconds.

### Claim 15 (depends on 3)

A method for manufacturing the grain-oriented electrical steel sheet according to claim 3, comprising:
a hot rolling process of heating and then hot-rolling a slab containing Si and Mn and obtaining a hot-rolled steel sheet;
a hot-band annealing process of performing hot-band annealing on the hot-rolled steel sheet and obtaining an annealed steel sheet;
a cold rolling process of cold-rolling the annealed steel sheet once or twice or more with intermediate annealing interposed therebetween and obtaining a cold-rolled steel sheet;
a decarburization annealing process of performing decarburization annealing on the cold-rolled steel sheet and obtaining a decarburization-annealed steel sheet;
a final annealing process of heating the decarburization-annealed steel sheet in a state which an annealing separator having a MgO content of 10 mass % to 50 mass % is applied to the surface of the decarburization-annealed steel sheet, then removing the annealing separator from the surface, and obtaining a final-annealed steel sheet;
an intermediate layer forming process of performing thermal oxidation annealing on the final-annealed steel sheet and forming an intermediate layer on a surface of the final-annealed steel sheet; and
an insulation coating forming process of forming an insulation coating on the intermediate layer,
wherein, in a cooling process of the final annealing process,
when a final annealing temperature is 1100° C. or higher, T1 is set to 1100° C., and when the final annealing temperature is less than 1100° C., T1 is set as the final annealing temperature,
cooling in a temperature range of T1 to 500° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.3 to 100000, and
in a cooling process of the insulation coating forming process,
cooling in a temperature range of 800° C. to 600° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.10 to 0.30 for a residence time of 10 seconds to 60 seconds.

### Claim 16 (depends on 4)

A method for manufacturing the grain-oriented electrical steel sheet according to claim 4, comprising:
a hot rolling process of heating and then hot-rolling a slab containing Si and Mn and obtaining a hot-rolled steel sheet;
a hot-band annealing process of performing hot-band annealing on the hot-rolled steel sheet and obtaining an annealed steel sheet;
a cold rolling process of cold-rolling the annealed steel sheet once or twice or more with intermediate annealing interposed therebetween and obtaining a cold-rolled steel sheet;
a decarburization annealing process of performing decarburization annealing on the cold-rolled steel sheet and obtaining a decarburization-annealed steel sheet;
a final annealing process of heating the decarburization-annealed steel sheet in a state which an annealing separator having a MgO content of 10 mass % to 50 mass % is applied to the surface of the decarburization-annealed steel sheet, then removing the annealing separator from the surface, and obtaining a final-annealed steel sheet;
an intermediate layer forming process of performing thermal oxidation annealing on the final-annealed steel sheet and forming an intermediate layer on a surface of the final-annealed steel sheet; and
an insulation coating forming process of forming an insulation coating on the intermediate layer,
wherein, in a cooling process of the final annealing process,
when a final annealing temperature is 1100° C. or higher, T1 is set to 1100° C., and when the final annealing temperature is less than 1100° C., T1 is set as the final annealing temperature,
cooling in a temperature range of T1 to 500° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.3 to 100000, and
in a cooling process of the insulation coating forming process,
cooling in a temperature range of 800° C. to 600° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.10 to 0.30 for a residence time of 10 seconds to 60 seconds.

### Claim 17 (depends on 5)

A method for manufacturing the grain-oriented electrical steel sheet according to claim 5, comprising:
a hot rolling process of heating and then hot-rolling a slab containing Si and Mn and obtaining a hot-rolled steel sheet;
a hot-band annealing process of performing hot-band annealing on the hot-rolled steel sheet and obtaining an annealed steel sheet;
a cold rolling process of cold-rolling the annealed steel sheet once or twice or more with intermediate annealing interposed therebetween and obtaining a cold-rolled steel sheet;
a decarburization annealing process of performing decarburization annealing on the cold-rolled steel sheet and obtaining a decarburization-annealed steel sheet;
a final annealing process of heating the decarburization-annealed steel sheet in a state which an annealing separator having a MgO content of 10 mass % to 50 mass % is applied to the surface of the decarburization-annealed steel sheet, then removing the annealing separator from the surface, and obtaining a final-annealed steel sheet;
an intermediate layer forming process of performing thermal oxidation annealing on the final-annealed steel sheet and forming an intermediate layer on a surface of the final-annealed steel sheet; and
an insulation coating forming process of forming an insulation coating on the intermediate layer,
wherein, in a cooling process of the final annealing process,
when a final annealing temperature is 1100° C. or higher, T1 is set to 1100° C., and when the final annealing temperature is less than 1100° C., T1 is set as the final annealing temperature,
cooling in a temperature range of T1 to 500° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.3 to 100000, and
in a cooling process of the insulation coating forming process,
cooling in a temperature range of 800° C. to 600° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.10 to 0.30 for a residence time of 10 seconds to 60 seconds.

### Claim 18 (depends on 6)

A method for manufacturing the grain-oriented electrical steel sheet according to claim 6, comprising:
a hot rolling process of heating and then hot-rolling a slab containing Si and Mn and obtaining a hot-rolled steel sheet;
a hot-band annealing process of performing hot-band annealing on the hot-rolled steel sheet and obtaining an annealed steel sheet;
a cold rolling process of cold-rolling the annealed steel sheet once or twice or more with intermediate annealing interposed therebetween and obtaining a cold-rolled steel sheet;
a decarburization annealing process of performing decarburization annealing on the cold-rolled steel sheet and obtaining a decarburization-annealed steel sheet;
a final annealing process of heating the decarburization-annealed steel sheet in a state which an annealing separator having a MgO content of 10 mass % to 50 mass % is applied to the surface of the decarburization-annealed steel sheet, then removing the annealing separator from the surface, and obtaining a final-annealed steel sheet;
an intermediate layer forming process of performing thermal oxidation annealing on the final-annealed steel sheet and forming an intermediate layer on a surface of the final-annealed steel sheet; and
an insulation coating forming process of forming an insulation coating on the intermediate layer,
wherein, in a cooling process of the final annealing process,
when a final annealing temperature is 1100° C. or higher, T1 is set to 1100° C., and when the final annealing temperature is less than 1100° C., T1 is set as the final annealing temperature,
cooling in a temperature range of T1 to 500° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.3 to 100000, and
in a cooling process of the insulation coating forming process,
cooling in a temperature range of 800° C. to 600° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.10 to 0.30 for a residence time of 10 seconds to 60 seconds.

### Claim 19 (depends on 2)

A method for manufacturing the grain-oriented electrical steel sheet according to claim 2, comprising:
a hot rolling process of heating and then hot-rolling a slab containing Si and Mn and obtaining a hot-rolled steel sheet;
a hot-band annealing process of performing hot-band annealing on the hot-rolled steel sheet and obtaining an annealed steel sheet;
a cold rolling process of cold-rolling the annealed steel sheet once or twice or more with intermediate annealing interposed therebetween and obtaining a cold-rolled steel sheet;
a decarburization annealing process of performing decarburization annealing on the cold-rolled steel sheet and obtaining a decarburization-annealed steel sheet;
a final annealing process of heating the decarburization-annealed steel sheet in a state which an annealing separator having a MgO content of 10 mass % to 50 mass % is applied to the surface of the decarburization-annealed steel sheet, then removing the annealing separator on the surface, and obtaining a final-annealed steel sheet; and
an intermediate layer and insulation coating forming process of forming an intermediate layer and an insulation coating on a surface of the final-annealed steel sheet in one process,
wherein, in a cooling process of the final annealing process,
when a final annealing temperature is 1100° C. or higher, T1 is set to 1100° C., and when the final annealing temperature is less than 1100° C., T1 is set as the final annealing temperature,
cooling in a temperature range of T1 to 500° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.3 to 100000,
in the intermediate layer and insulation coating forming process,
an atmosphere in a temperature range of 800° C. to 1150° C. is set to an oxidation degree (PH2O/PH2) of 0.05 to 0.18, and
in a cooling process of the intermediate layer and insulation coating forming process,
cooling in a temperature range of 800° C. to 600° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.10 to 0.30 for a residence time of 10 seconds to 60 seconds.

### Claim 20 (depends on 3)

A method for manufacturing the grain-oriented electrical steel sheet according to claim 3, comprising:
a hot rolling process of heating and then hot-rolling a slab containing Si and Mn and obtaining a hot-rolled steel sheet;
a hot-band annealing process of performing hot-band annealing on the hot-rolled steel sheet and obtaining an annealed steel sheet;
a cold rolling process of cold-rolling the annealed steel sheet once or twice or more with intermediate annealing interposed therebetween and obtaining a cold-rolled steel sheet;
a decarburization annealing process of performing decarburization annealing on the cold-rolled steel sheet and obtaining a decarburization-annealed steel sheet;
a final annealing process of heating the decarburization-annealed steel sheet in a state which an annealing separator having a MgO content of 10 mass % to 50 mass % is applied to the surface of the decarburization-annealed steel sheet, then removing the annealing separator on the surface, and obtaining a final-annealed steel sheet; and
an intermediate layer and insulation coating forming process of forming an intermediate layer and an insulation coating on a surface of the final-annealed steel sheet in one process,
wherein, in a cooling process of the final annealing process,
when a final annealing temperature is 1100° C. or higher, T1 is set to 1100° C., and when the final annealing temperature is less than 1100° C., T1 is set as the final annealing temperature,
cooling in a temperature range of T1 to 500° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.3 to 100000,
in the intermediate layer and insulation coating forming process,
an atmosphere in a temperature range of 800° C. to 1150° C. is set to an oxidation degree (PH2O/PH2) of 0.05 to 0.18, and
in a cooling process of the intermediate layer and insulation coating forming process,
cooling in a temperature range of 800° C. to 600° C. is performed in an atmosphere of an oxidation degree (PH2O/PH2) of 0.10 to 0.30 for a residence time of 10 seconds to 60 seconds.