# US 2022/0037654 A1 · Zinc foil, primary battery negative electrode active material using same, and zinc foil production method

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0037654 A1
- Document ID: US20220037654A1
- Status: Published application
- Kind: A1
- Application number: 17/279,007
- Filed: 2019-10-01
- Published: 2022-02-03
- Earliest claimed: 2018-10-03
- Assignees: Mitsui Mining & Smelting Co., Ltd.
- Applicants: Mitsui Mining & Smelting Co., Ltd.
- Inventors: Tsuneyoshi KAMADA; Naoki KUMADA; Masashi SAKANO; Hidetoshi INOUE; Hideyuki NAGAOKA; Yasuhiro OCHI
- Web page: https://patentgrep.com/patent/US20220037654A1

## CPC

- C22F 1/165: {of zinc or cadmium or alloys based thereon}
- H01M 4/42: Alloys based on zinc
- C22C 18/00: Alloys based on zinc
- C25D 1/04: Wires; Strips; Foils
- C25D 3/22: of zinc
- C25D 3/565: {containing more than 50% by weight of zinc}
- H01M 4/06: Electrodes for primary cells
- Y02E 60/10: Energy storage using batteries
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

A zinc foil is provided that can be used as a negative electrode active material, and in a battery including the zinc foil as a negative electrode active material, the amount of gas generated during long term storage of the battery is reduced as compared with that in a battery including a conventional zinc foil. The zinc foil contains zinc as a main material and bismuth. The bismuth content is 100 ppm or more and 10000 ppm or less on a mass basis. The zinc crystal grain size is 0.2 μm or more and 8 μm or less. The bismuth crystal grain size is less than 1000 nm, as measured in a backscattered electron image obtained using a scanning electron microscope. The zinc foil is free of aluminum and/or lead, or even if the zinc foil contains aluminum and/or lead, the aluminum content is 1% or less on a mass basis and/or the lead content is 200 ppm or less on a mass basis.

## Claims

### Claim 1

A zinc foil comprising zinc as a main material and bismuth,
the zinc foil having a bismuth content of 100 ppm or more and 10000 ppm or less on a mass basis, and a zinc crystal grain size of 0.2 μm or more and 8 μm or less.

### Claim 2 (depends on 1)

The zinc foil according to claim 1,
wherein, in a bismuth mapping image with a virtual grid of squares each having a side length of 300 nm, bismuth is observed in 2% N or more of the squares relative to a total number of the squares, the bismuth mapping image being obtained by energy dispersive X-ray spectroscopy using a scanning electron microscope.

### Claim 3 (depends on 1)

The zinc foil according to claim 1,
wherein a bismuth crystal grain size is less than 1000 nm, as measured in a backscattered electron image obtained using a scanning electron microscope.

### Claim 4 (depends on 1)

The zinc foil according to claim 1,
wherein the zinc foil is free of aluminum and/or lead, or even if the zinc foil contains aluminum and/or lead, an aluminum content is 1% or less on a mass basis and/or a lead content is 200 ppm or less on a mass basis.

### Claim 5 (depends on 1)

The zinc foil according to claim 1,
wherein the bismuth content is 150 ppm or more and 6000 ppm or less on a mass basis.

### Claim 6 (depends on 1)

The zinc foil according to claim 1,
wherein the zinc foil further contains at least one element selected from the group consisting of indium, magnesium, calcium, gallium, tin, barium, and strontium, and
a total content of the at least one element is 10 ppm or more and 10000 ppm or less on a mass basis.

### Claim 7 (depends on 1)

The zinc foil according to claim 1,
wherein the zinc foil has a folding endurance of 10 or more, in terms of the number of double bending operation, as determined in accordance with JIS P8115.

### Claim 8

A negative electrode active material for a primary battery, comprising a zinc foil,
the zinc foil comprising zinc as a main material and bismuth,
the zinc foil having a bismuth content of 100 ppm or more and 10000 ppm or less on a mass basis, and a zinc crystal grain size of 0.2 μm or more and 8 μm or less.

### Claim 9 (depends on 8)

The negative electrode active material for a primary battery according to claim 8,
wherein, in a bismuth mapping image with a virtual grid of squares each having a side length of 300 nm, bismuth is observed in 2% N or more of the squares relative to a total number of the squares, the bismuth mapping image being obtained by energy dispersive X-ray spectroscopy using a scanning electron microscope.

### Claim 10 (depends on 8)

The negative electrode active material for a primary battery according to claim 8,
wherein a bismuth crystal grain size is less than 1000 nm, as measured in a backscattered electron image obtained using a scanning electron microscope.

### Claim 11 (depends on 1)

The negative electrode active material for a primary battery according to claim 1,
wherein the zinc foil is free of aluminum and/or lead, or even if the zinc foil contains aluminum and/or lead, an aluminum content is 1% or less on a mass basis and/or a lead content is 200 ppm or less.

### Claim 12

A method for producing a zinc foil, the method comprising:
precipitating a zinc foil containing zinc as a main material and bismuth through reduction on a cathode immersed in an electrolyte solution containing a zinc source and a bismuth source,
wherein a current density in the reduction is 1000 A/m2 or more and 10000 A/m2 or less;
a dimensionally stable electrode is used as an anode, and
the electrolyte solution has a bismuth content of 200 ppm or more and 10000 ppm or less, on a mass basis, relative to a total mass of zinc and bismuth in the electrolyte solution.