# US 2022/0033988 A1 · Ni-PLATED STEEL SHEET AND METHOD FOR MANUFACTURING Ni-PLATED STEEL SHEET

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0033988 A1
- Document ID: US20220033988A1
- Status: Published application
- Kind: A1
- Application number: 17/296,395
- Filed: 2019-12-20
- Published: 2022-02-03
- Earliest claimed: 2018-12-27
- Assignees: Nippon Steel Corporation
- Applicants: Nippon Steel Corporation
- Inventors: Yasuto GOTO; Kiyokazu ISHIZUKA; Takehiro TAKAHASHI
- Web page: https://patentgrep.com/patent/US20220033988A1

## CPC

- C25D 5/617: {Crystalline layers}
- B32B 15/013: {one layer being formed of an iron alloy or steel, another layer being formed of a metal other than iron or aluminium}
- B32B 15/015: {the said other metal being copper or nickel or an alloy thereof}
- C21D 1/26: Methods of annealing
- C21D 9/46: for sheet metals
- C22C 19/03: based on nickel
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C25D 3/12: of nickel or cobalt
- C25D 5/14: two or more layers being of nickel or chromium, e.g. duplex or triplex layers
- C25D 5/18: Electroplating using modulated, pulsed or reversing current
- C25D 5/50: by heat-treatment
- Y02E 60/10: Energy storage using batteries
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

A Ni-plated steel sheet according to an aspect of the present invention includes: a base steel sheet; an Fe—Ni diffusion alloy region disposed on the base steel sheet; and a Ni plating region disposed on the Fe—Ni diffusion alloy region, in which an average equivalent circle diameter of crystal grains made of Ni (fcc) in the Ni plating region measured in a cross section perpendicular to a rolled surface of the base steel sheet is 0.2 to 4.0 μm.

## Claims

### Claim 1

A Ni-plated steel sheet, comprising:
a base steel sheet;
an Fe—Ni diffusion alloy region disposed on the base steel sheet; and
a Ni plating region disposed on the Fe—Ni diffusion alloy region,
wherein an average equivalent circle diameter of crystal grains made of Ni (fcc) in the Ni plating region measured in a cross section perpendicular to a rolled surface of the base steel sheet is 0.2 to 4.0 μm.

### Claim 2 (depends on 1)

The Ni-plated steel sheet according to claim 1,
wherein a value obtained by dividing the average equivalent circle diameter of the crystal grains made of the Ni (fcc) in the Ni plating region by a thickness of the Ni plating region is 0.50 to 2.00.

### Claim 3 (depends on 1)

The Ni-plated steel sheet according to claim 1,
wherein a Ni coating weight per one surface in the Fe—Ni diffusion alloy region and the Ni plating region is 1.5 to 65 g/m2.

### Claim 4 (depends on 1)

A method for manufacturing the Ni-plated steel sheet according to claim 1, the method comprising:
electrolytic Ni plating on a base steel sheet to obtain a Ni-plated steel sheet material; and
annealing the Ni-plated steel sheet material,
wherein the electrolytic Ni plating includes three or more on-times and off-times between the on-times,
an average current density per one surface of the base steel sheet in each of the on-times is set to 200 A/m2 to 3,500 A/m2,
an amount of charge per one surface of the base steel sheet in each of the on-times is set to 800 C/m2 to 40,000 C/m2,
in each of the on-times, a current density is set to be inconstant, and a maximum current density per one surface of the base steel sheet is set to be higher than the average current density per one surface of the base steel sheet by 7% or more and is set to 4,000 A/m2 or less,
a soaking temperature in the annealing is set to 650° C. or higher and 850° C. or lower, and
a soaking time in the annealing is set to 10 seconds or longer and 109 seconds or shorter.

### Claim 5 (depends on 4)

The method for manufacturing the Ni-plated steel sheet according to claim 4,
wherein a length of each of the off-times is 0.1 seconds or longer.

### Claim 6 (depends on 2)

The Ni-plated steel sheet according to claim 2,
wherein a Ni coating weight per one surface in the Fe—Ni diffusion alloy region and the Ni plating region is 1.5 to 65 g/m2.

### Claim 7 (depends on 2)

A method for manufacturing the Ni-plated steel sheet according to claim 2, the method comprising:
electrolytic Ni plating on a base steel sheet to obtain a Ni-plated steel sheet material; and
annealing the Ni-plated steel sheet material,
wherein the electrolytic Ni plating includes three or more on-times and off-times between the on-times,
an average current density per one surface of the base steel sheet in each of the on-times is set to 200 A/m2 to 3,500 A/m2,
an amount of charge per one surface of the base steel sheet in each of the on-times is set to 800 C/m2 to 40,000 C/m2,
in each of the on-times, a current density is set to be inconstant, and a maximum current density per one surface of the base steel sheet is set to be higher than the average current density per one surface of the base steel sheet by 7% or more and is set to 4,000 A/m2 or less,
a soaking temperature in the annealing is set to 650° C. or higher and 850° C. or lower, and
a soaking time in the annealing is set to 10 seconds or longer and 109 seconds or shorter.

### Claim 8 (depends on 3)

A method for manufacturing the Ni-plated steel sheet according to claim 3, the method comprising:
electrolytic Ni plating on a base steel sheet to obtain a Ni-plated steel sheet material; and
annealing the Ni-plated steel sheet material,
wherein the electrolytic Ni plating includes three or more on-times and off-times between the on-times,
an average current density per one surface of the base steel sheet in each of the on-times is set to 200 A/m2 to 3,500 A/m2,
an amount of charge per one surface of the base steel sheet in each of the on-times is set to 800 C/m2 to 40,000 C/m2,
in each of the on-times, a current density is set to be inconstant, and a maximum current density per one surface of the base steel sheet is set to be higher than the average current density per one surface of the base steel sheet by 7% or more and is set to 4,000 A/m2 or less,
a soaking temperature in the annealing is set to 650° C. or higher and 850° C. or lower, and
a soaking time in the annealing is set to 10 seconds or longer and 109 seconds or shorter.

### Claim 9 (depends on 6)

A method for manufacturing the Ni-plated steel sheet according to claim 6, the method comprising:
electrolytic Ni plating on a base steel sheet to obtain a Ni-plated steel sheet material; and
annealing the Ni-plated steel sheet material,
wherein the electrolytic Ni plating includes three or more on-times and off-times between the on-times,
an average current density per one surface of the base steel sheet in each of the on-times is set to 200 A/m2 to 3,500 A/m2,
an amount of charge per one surface of the base steel sheet in each of the on-times is set to 800 C/m2 to 40,000 C/m2,
in each of the on-times, a current density is set to be inconstant, and a maximum current density per one surface of the base steel sheet is set to be higher than the average current density per one surface of the base steel sheet by 7% or more and is set to 4,000 A/m2 or less,
a soaking temperature in the annealing is set to 650° C. or higher and 850° C. or lower, and
a soaking time in the annealing is set to 10 seconds or longer and 109 seconds or shorter.

### Claim 10 (depends on 7)

The method for manufacturing the Ni-plated steel sheet according to claim 7,
wherein a length of each of the off-times is 0.1 seconds or longer.

### Claim 11 (depends on 8)

The method for manufacturing the Ni-plated steel sheet according to claim 8,
wherein a length of each of the off-times is 0.1 seconds or longer.

### Claim 12 (depends on 9)

The method for manufacturing the Ni-plated steel sheet according to claim 9,
wherein a length of each of the off-times is 0.1 seconds or longer.