# US 2022/0033940 A1 · Non-grain oriented electrical steel and method for manufacturing same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0033940 A1
- Document ID: US20220033940A1
- Status: Published application
- Kind: A1
- Application number: 17/280,376
- Filed: 2019-05-23
- Published: 2022-02-03
- Earliest claimed: 2018-09-27
- Assignees: Posco
- Applicants: Posco
- Inventors: Jae-Song Kim; Seung Il Kim; Jae Kim; Su-Yong Shin; Yong-Soo Kim
- Web page: https://patentgrep.com/patent/US20220033940A1

## CPC

- C22C 38/004: {Very low carbon steels, i.e. having a carbon content of less than 0,01%}
- C22C 38/38: with more than 1.5% by weight of manganese
- C21D 1/30: Stress-relieving
- C21D 6/00: Heat treatment of ferrous alloys
- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/12: during manufacturing of articles with special electromagnetic properties
- C21D 8/1244: characterised by the heat treatment
- C21D 8/1261: {following hot rolling}
- C21D 8/1283: {Application of a separating or insulating coating}
- C21D 9/46: for sheet metals
- C22C 38/00: Ferrous alloys, e.g. steel alloys (cast-iron alloys C22C37/00)
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/20: with copper
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/34: with more than 1.5% by weight of silicon
- H01F 1/147: Alloys characterised by their composition {(treatment thereof for enhancing their electromagnetic properties C21D8/12)}
- Y02P 10/20: Recycling
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

A non-oriented electrical steel sheet according to an embodiment of the present invention includes: in wt %, C at 0.004 wt % or less (excluding 0 wt %), Si at 2.5 to 4.0 wt %, P at 0.1 wt % or less (excluding 0 wt %), Al at 0.3 to 2.0 wt %, N at 0.003 wt % or less (excluding 0 wt %), S at 0.003 wt % or less (excluding 0 wt %), Mn at 0.15 to 2.5 wt %, Cr at 0.5 wt % (excluding 0 wt %), and the balance including Fe and other impurities unavoidably added thereto; satisfies the following Equation 1; and has an average grain size of 20 μm or less. [Mn]≥1450×[S]−0.8 [Equation 1] (In Equation 1, [Mn] and [S] represent a content (wt %) of Mn and S, respectively.)

## Claims

### Claim 1

A non-oriented electrical steel sheet, comprising:
in wt %, C at 0.004 wt % or less (excluding 0 wt %), Si at 2.5 to 4.0 wt %, P at 0.1 wt % or less (excluding 0 wt %), Al at 0.3 to 2.0 wt %, N at 0.003 wt % or less (excluding 0 wt %), S at 0.003 wt % or less (excluding 0 wt %), Mn at 0.15 to 2.5 wt %, Cr at 0.5 wt % (excluding 0 wt %), and the balance including Fe and other impurities unavoidably added thereto;
satisfying Equation 1 below; and
having an average grain size of 20 μm or less:
[Mn]≥1450×[S]−0.8 [Equation 1]
(in Equation 1, [Mn] and [S] represent a content (wt %) of Mn and S, respectively.)

### Claim 2 (depends on 1)

The non-oriented electrical steel sheet of claim 1, further comprising
one or more of Ti at 0.003 wt % or less, Nb at 0.003 wt % or less, and Cu at 0.1 wt % or less.

### Claim 3 (depends on 1)

The non-oriented electrical steel sheet of claim 1, wherein
a density of sulfide having a diameter of 1 nm to 0.1 μm is 250,000/mm2 or less.

### Claim 4 (depends on 3)

The non-oriented electrical steel sheet of claim 3, wherein
the sulfide includes MnS, MnS, or CuS.

### Claim 5 (depends on 1)

The non-oriented electrical steel sheet of claim 1, wherein
a magnetic flux density (B50) induced in a magnetic field of 5000 is 1.61 T or more, and the non-oriented electrical steel sheet has a yield strength of 500 MPa or more.

### Claim 6 (depends on 1)

The non-oriented electrical steel sheet of claim 1, wherein
iron loss (W10/400) measured after stress relief annealing that is performed at a temperature of 750° C. for 2 hours is 12 W/kg or less.

### Claim 7

A manufacturing method of a non-oriented electrical steel sheet, comprising:
heating a slab that includes, in wt %, C at 0.004 wt % or less (excluding 0 wt %), Si at 2.5 to 4.0 wt %, P at 0.1 wt % or less (excluding 0 wt %), Al at 0.3 to 2.0 wt %, N at 0.003 wt % or less (excluding 0 wt %), S at 0.003 wt % or less (excluding 0 wt %), Mn at 0.15 to 2.5 wt %, Cr at 0.5 wt % (excluding 0 wt %), and the balance including Fe and other impurities unavoidably added thereto and that satisfies Equation 1 below;
hot-rolling the slab to manufacture a hot rolled sheet;
cold rolling the hot rolled sheet to manufacture a cold rolled sheet; and
final annealing the cold rolled sheet at a temperature of 710 to 820° C.
[Mn]≥1450×[S]−0.8 [Equation 1]
(in Equation 1, [Mn] and [S] represent a content (wt %) of Mn and S, respectively.)

### Claim 8 (depends on 7)

The manufacturing method of the non-oriented electrical steel sheet of claim 7, wherein
the slab further includes one or more of Ti at 0.003 wt % or less, Nb at 0.003 wt % or less, and Cu at 0.1 wt % or less.

### Claim 9 (depends on 7)

The manufacturing method of the non-oriented electrical steel sheet of claim 7, wherein
the slab is heated at 1100° C. to 1250° C.

### Claim 10 (depends on 7)

The manufacturing method of the non-oriented electrical steel sheet of claim 7, further comprising
after the manufacturing of the hot rolled sheet, annealing the hot rolled sheet at a temperature of 850 to 1200° C.

### Claim 11 (depends on 7)

The manufacturing method of the non-oriented electrical steel sheet of claim 7, further comprising
after the final annealing, stress relief annealing that is performed in a temperature range of 700 to 900° C.