# US 2022/0033654 A1 · Thermally stable and electrically isolating barrier film

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0033654 A1
- Document ID: US20220033654A1
- Status: Published application
- Kind: A1
- Application number: 17/412,424
- Filed: 2021-08-26
- Published: 2022-02-03
- Earliest claimed: 2017-10-09
- Assignees: Corning Incorporated
- Applicants: Corning Incorporated
- Inventors: Arthur Winston Martin; Shawn Michael O'Malley
- Web page: https://patentgrep.com/patent/US20220033654A1

## CPC

- C08L 79/08: Polyimides; Polyester-imides; Polyamide-imides; Polyamide acids or similar polyimide precursors
- C08G 73/1014: {in the form of (mono)anhydrid}
- C08G 73/1039: {comprising halogen-containing substituents}
- C08G 77/045: {containing less than 25 silicon atoms}
- C08K 5/1515: Three-membered rings
- C08K 5/5419: containing at least one Si—C bond
- C08K 9/04: Ingredients treated with organic substances {(treated with macromolecular compounds C08K9/08)}
- C09D 179/08: Polyimides; Polyester-imides; Polyamide-imides; Polyamide acids or similar polyimide precursors
- C09D 183/04: Polysiloxanes
- C08K 2201/011: Nanostructured additives
- C08L 2201/08: Stabilised against heat, light or radiation or oxydation
- C08L 2203/16: used for films
- C08L: COMPOSITIONS OF MACROMOLECULAR COMPOUNDS (compositions based on polymerisable monomers C08F, C08G; artificial filaments or fibres D01F; textile treating compositions D06)
- C08G: MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
- C08K: Use of inorganic or non-macromolecular organic substances as compounding ingredients (paints, inks, varnishes, dyes, polishes, adhesives C09)
- C09D: COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR (cosmetics A61K; processes for applying liquids or other fluent materials to surfaces, in general, B05D; staining wood B27K5/02; glazes or vitreous enamels C03C; natural resins, French polish, drying-oils, driers, turpentine, per se, C09F; polishing compositions other than French polish, ski waxes C09G; adhesives or use of materials as adhesives C09J; materials for sealing or packing joints or covers C09K3/10; materials for stopping leaks C09K3/12; processes for the electrolytic or electrophoretic production of coatings C25D)

## Abstract

A thermoset barrier film including: a reaction product of the formulas (I), (II), (III), (IV), or a mixture thereof, as defined herein. Also disclosed are methods of making and using the thermoset barrier film, and devices incorporating the thermoset barrier film.

## Claims

### Claim 1

A thermoset barrier film, comprising:
a reaction product comprising:
a fluorinated polyimide oligomer having anhydride end caps, in from 50 to 90 wt %;
a cross-linker, in from 1 to 40 wt %, comprising a polyhedral oligomeric silsesquioxane having at least one pendant group selected from an epoxy group, a di-aryl group, an acrylate group, or mixtures thereof;
a tie agent having at least one of each of an acrylate group and an epoxy group, in from 0.1 to 20 wt %;
an epoxy silane adhesion promoter, in from 0.1 to 3 wt %; and
an initiator, in from 1 to 20 wt %, based on a total of 100 wt % of the barrier film, wherein the barrier film is electrically isolating and has a voltage breakdown of from 300 to 1900 volts per micron,
wherein the barrier film is thermally stable up to at least 250° C. with no loss in mass below 250° C., and
further wherein the barrier film has a water contact angle of from 89 degrees to 112 degrees.

### Claim 2 (depends on 1)

The barrier film of claim 1, further comprising:
a surface modified nano-silica having a primary particle size of from about 10 nm to 20 nm in a total amount of from 5 to 30 wt % by superaddition, wherein the barrier film has a pencil hardness of at least 7 H.

### Claim 3 (depends on 2)

The barrier film of claim 2, wherein the cross-linker is in from 8 to 40 wt %.

### Claim 4 (depends on 1)

The barrier film of claim 1, further comprising:
at least one fluorine booster compound selected from a fluorinated urethane-acrylate of formula, a fluorinated epoxy, or a mixture thereof, in a total amount of from 0.1 to 30 wt % by superaddition.

### Claim 5 (depends on 4)

The barrier film of claim 4, wherein the fluorinated polyimide oligomer is in from 50 to 54 wt %, the cross-linker is in from about 14 to 18 wt %, the tie agent is in from about 5 to 8 wt %, the epoxy silane adhesion promoter is in from about 1.5 to 4 wt %, and the initiator is in from about 2 to 5 wt %, and further wherein the at least one fluorine booster compound is in from about 15 to 30 wt % by superaddition.

### Claim 6 (depends on 5)

The barrier film of claim 5, wherein the barrier film is electrically isolating and has a voltage breakdown of from 1000 to 1200 volts per micron, and further wherein the barrier film has a water contact angle of at least about 112 degrees.

### Claim 7 (depends on 1)

The barrier film of claim 1, wherein the fluorinated polyimide oligomer is in from 62 to 68 wt %, the cross-linker is in from about 17 to 23 wt %, the tie agent is in from about 6 to 10 wt %, the epoxy silane adhesion promoter is in from about 1.5 to 4.5 wt %, and the initiator is in from about 3 to 6 wt %.

### Claim 8 (depends on 7)

The barrier film of claim 7, wherein the barrier film is electrically isolating and has a voltage breakdown of from 750 to 900 volts per micron.

### Claim 9

A pourable formulation for a thermoset barrier film, comprising:
a solvent or a liquid vehicle; and
a reaction product dissolved in the solvent or suspended in the liquid vehicle,
wherein the reaction product comprises:
a fluorinated polyimide oligomer having anhydride end caps, in from 50 to 90 wt %;
a cross-linker, in from 1 to 40 wt %, comprising a polyhedral oligomeric silsesquioxane having at least one pendant group selected from an epoxy group, a di-aryl group, an acrylate group, or mixtures thereof;
a tie agent having at least one of each of an acrylate group and an epoxy group, in from 0.1 to 20 wt %;
an epoxy silane adhesion promoter, in from 0.1 to 3 wt %; and
an initiator, in from 1 to 20 wt %, based on a total of 100 wt % of the barrier film.

### Claim 10 (depends on 9)

The formulation of claim 9, further comprising:
a surface modified nano-silica having a primary particle size of from about 10 nm to 20 nm in a total amount of from 5 to 30 wt % by superaddition, wherein the barrier film has a pencil hardness of at least 7 H.

### Claim 11 (depends on 10)

The formulation of claim 10, wherein the cross-linker is in from 8 to 40 wt %.

### Claim 12 (depends on 9)

The formulation of claim 9, further comprising:
at least one fluorine booster compound selected from a fluorinated urethane-acrylate of formula, a fluorinated epoxy, or a mixture thereof, in a total amount of from 0.1 to 30 wt % by superaddition.

### Claim 13 (depends on 12)

The formulation of claim 12, wherein the fluorinated polyimide oligomer is in from 50 to 54 wt %, the cross-linker is in from about 14 to 18 wt %, the tie agent is in from about 5 to 8 wt %, the epoxy silane adhesion promoter is in from about 1.5 to 4 wt %, and the initiator is in from about 2 to 5 wt %, and further wherein the at least one fluorine booster compound is in from about 15 to 30 wt % by superaddition.

### Claim 14 (depends on 9)

The formulation of claim 9, wherein the fluorinated polyimide oligomer is in from 62 to 68 wt %, the cross-linker is in from about 17 to 23 wt %, the tie agent is in from about 6 to 10 wt %, the epoxy silane adhesion promoter is in from about 1.5 to 4.5 wt %, and the initiator is in from about 3 to 6 wt %.

### Claim 15

A method of making a thermoset barrier film, comprising:
combining a reaction product, the reaction product comprising:
a fluorinated polyimide oligomer having anhydride end caps, in from 50 to 90 wt %;
a cross-linker, in from 1 to 40 wt %, comprising a polyhedral oligomeric silsesquioxane having at least one pendant group selected from an epoxy group, a di-aryl group, an acrylate group, or mixtures thereof;
a tie agent having at least one of each of an acrylate group and an epoxy group, in from 0.1 to 20 wt %;
an epoxy silane adhesion promoter, in from 0.1 to 3 wt %; and
an initiator, in from 1 to 20 wt %, based on a total of 100 wt % of the thermoset barrier film;
initiating a reaction of the reaction product after the combining step for a time using radiation, heat or a combination thereof; and
coating the reaction product on a substrate after the initiating step to form a thermoset barrier film on the substrate.

### Claim 16 (depends on 15)

The method of claim 15, wherein the reaction product of the combining step further comprises:
a surface modified nano-silica having a primary particle size of from about 10 nm to 20 nm in a total amount of from 5 to 30 wt % by superaddition, wherein the barrier film has a pencil hardness of at least 7 H.

### Claim 17 (depends on 15)

The method of claim 15, wherein the reaction product of the combining step further comprises:
at least one fluorine booster compound selected from a fluorinated urethane-acrylate of formula, a fluorinated epoxy, or a mixture thereof, in a total amount of from 0.1 to 30 wt % by superaddition.

### Claim 18 (depends on 17)

The method of claim 17, wherein the fluorinated polyimide oligomer is in from 50 to 54 wt %, the cross-linker is in from about 14 to 18 wt %, the tie agent is in from about 5 to 8 wt %, the epoxy silane adhesion promoter is in from about 1.5 to 4 wt %, and the initiator is in from about 2 to 5 wt %, and further wherein the at least one fluorine booster compound is in from about 15 to 30 wt % by superaddition.

### Claim 19 (depends on 15)

The method of claim 15, wherein the fluorinated polyimide oligomer is in from 62 to 68 wt %, the cross-linker is in from about 17 to 23 wt %, the tie agent is in from about 6 to 10 wt %, the epoxy silane adhesion promoter is in from about 1.5 to 4.5 wt %, and the initiator is in from about 3 to 6 wt %.

### Claim 20 (depends on 15)

The method of claim 15, wherein the thermoset barrier film is electrically isolating and has a voltage breakdown of from 300 to 1900 volts per micron, wherein the barrier film is thermally stable up to at least 250° C. with no loss in mass below 250° C., and further wherein the barrier film has a water contact angle of from 89 degrees to 112 degrees.