# US 2022/0032364 A1 · Die casting method for filtering cavity

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0032364 A1
- Document ID: US20220032364A1
- Status: Published application
- Kind: A1
- Application number: 17/413,762
- Filed: 2019-12-02
- Published: 2022-02-03
- Earliest claimed: 2018-12-14
- Assignees: Zhuhai Runxingtai Electrical Co., Ltd.
- Applicants: Zhuhai Runxingtai Electrical Co., Ltd
- Inventors: Ying ZHANG; Jie TAN; Jicheng WANG; Gunan LI; Ziqiang HUANG; Huaide REN
- Web page: https://patentgrep.com/patent/US20220032364A1

## CPC

- B22D 17/32: Controlling equipment
- B22D 43/004: {by using filtering means (B22C9/086 takes precedence)}
- B22D 1/00: Treatment of fused masses in the ladle or the supply runners before casting {(for continuous casting B22D11/10; metallurgical processing, e.g. refining of iron or other metal C21, C22, C25C)}
- B22D 17/007: {Semi-solid pressure die casting}
- B22D 27/02: Use of electric or magnetic effects {(for continuous casting B22D11/015, B22D11/11)}
- B22F 1/148: Agglomerating
- C22F 1/04: of aluminium or alloys based thereon
- B22F 9/08: by casting, e.g. through sieves or in water, by atomising or spraying (using electric discharge B22F9/14)
- B22D: CASTING OF METALS; CASTING OF OTHER SUBSTANCES BY THE SAME PROCESSES OR DEVICES (shaping of plastics or substances in a plastic state B29C; metallurgical processing, selection of substances to be added to metal C21, C22)
- B22F: WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER (making alloys by powder metallurgy C22C); APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)

## Abstract

A die casting method includes stirring an aluminum alloy liquid in a stirrer under an airtight vacuum condition. The stirrer includes an electromagnetic inductor and a stirring rod. The aluminum alloy liquid is simultaneously subjected to an electromagnetic stirring in a direction of a magnetic field generated by the electromagnetic inductor and a mechanical stirring under a rotation action of the stirring rod. The aluminum alloy liquid is stirred for 20-80 minutes until the aluminum alloy liquid becomes semisolid to obtain a semisolid aluminum alloy slurry. The method further includes injecting the semisolid aluminum alloy slurry into a filter die to perform die casting molding at an injection speed of 1.5-2.5 m/s, an injection specific pressure of 30-80 MPa, a pressurization pressure of 60-80 MPa, and a temperature of the filter die of 250-400° C., and maintaining pressure for 7-30 seconds to obtain the filtering cavity.

## Claims

### Claim at position 1

-10. (canceled)

### Claim 11

A die casting method for a filtering cavity comprising:
transferring an aluminum alloy liquid to a stirrer including:
an electromagnetic inductor; and
a stirring rod arranged across an inside of the stirrer;
covering the stirrer and evacuating air inside the stirrer;
starting the stirrer to stir the aluminum alloy liquid under an airtight vacuum condition, the aluminum alloy liquid being simultaneously subjected to:
an electromagnetic stirring in a direction of a magnetic field generated by the electromagnetic inductor; and
a mechanical stirring under a rotation action of the stirring rod;
continuing stirring the aluminum alloy liquid for 20-80 minutes until the aluminum alloy liquid becomes semisolid to obtain a semisolid aluminum alloy slurry, a temperature of the semisolid aluminum alloy slurry being 550-650° C.; and
injecting the semisolid aluminum alloy slurry into a filter die to perform die casting molding at an injection speed of 1.5-2.5 m/s, an injection specific pressure of 30-80 MPa, a pressurization pressure of 60-80 MPa, and a temperature of the filter die of 250-400° C., and maintaining pressure for 7-30 seconds to obtain the filtering cavity.

### Claim 12 (depends on 11)

The die casting method according to claim 11, wherein injecting the semisolid aluminum alloy slurry into the filter die to perform die casting and maintaining pressure includes:
preparing the filter die and spraying a lubricant into a die cavity of the filter die;
injecting the semisolid aluminum alloy slurry into the filter die at an injection pressure of 100-175 MPa, the injection speed of 1.5-2.5 m/s, the injection specific pressure of 30-50 MPa, and the pressurization pressure of 60-80 MPa to perform die casting molding; and
after the die casting molding, keeping the pressure at 100-175 MPa for 7-15 seconds until a casting of the filtering cavity is solidified, and then cooling to obtain the filtering cavity.

### Claim 13 (depends on 12)

The die casting method according to claim 12, further comprising, before transferring the aluminum alloy liquid to the stirrer:
preparing an aluminum alloy; and
heating the aluminum alloy to melt to obtain the aluminum alloy liquid with a temperature of 700-750° C.

### Claim 14 (depends on 13)

The die casting method according to claim 13, further comprising, before transferring the aluminum alloy liquid to the stirrer:
placing the aluminum alloy liquid obtained by melting the aluminum alloy into a spraying device;
carrying out powder spraying refining with inert gas as a carrier perform primary degassing to remove bubbles in the aluminum alloy liquid for a refining time of 8-18 minutes; and
filtering the aluminum alloy liquid after letting the aluminum alloy liquid stand for 15-30 minutes after refining.

### Claim 15 (depends on 14)

The die casting method according to claim 14, further comprising, before transferring the aluminum alloy liquid to the stirrer:
transferring the aluminum alloy liquid refined by powder spraying to a rotor degassing device; and
blowing nitrogen into the aluminum alloy liquid for secondary degassing with a rotor speed of the rotor degassing device being 500-600 rpm.

### Claim 16 (depends on 11)

The die casting method according to claim 11, wherein the mechanical stirring by the stirring rod includes a repeated rotary stirring from a center of the stirrer to an edge of the stirrer.

### Claim 17 (depends on 16)

The die casting method according to claim 16, wherein the mechanical stirring by the stirring rod further includes stirring up and down.

### Claim 18 (depends on 11)

The die casting method according to claim 11, wherein the mechanical stirring by the stirring rod includes stirring up and down.

### Claim 19 (depends on 11)

The die casting method according to claim 11, wherein the stirring rod includes a graphite stirring rod.

### Claim 20 (depends on 11)

The die casting method according to claim 11, wherein the magnetic field generated by the electromagnetic inductor of the stirrer includes at least one of a rotating magnetic field or a traveling wave magnetic field.

### Claim 21 (depends on 11)

The die casting method according to claim 11, further comprising, after the filtering cavity is obtained:
subjecting the filtering cavity after the die cast molding to solution treatment at 545-550° C. for 6-8 hours; and
water quenching the filtering cavity after the solution treatment.

### Claim 22 (depends on 21)

The die casting method according to claim 21, further comprising, after water quenching:
subjecting the filtering cavity quenched in water to aging treatment at 185-250° C. for 3-5 hours.