# US 2022/0017984 A1 · Ferritic stainless steel sheet and method for producing same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2022/0017984 A1
- Document ID: US20220017984A1
- Status: Published application
- Kind: A1
- Application number: 17/299,308
- Filed: 2019-11-27
- Published: 2022-01-20
- Earliest claimed: 2018-12-11
- Assignees: Jfe Steel Corporation
- Applicants: Jfe Steel Corporation
- Inventors: Keishi INOUE; Hidetaka KAWABE; Masataka YOSHINO; Mitsuyuki FUJISAWA
- Web page: https://patentgrep.com/patent/US20220017984A1

## CPC

- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C21D 9/46: for sheet metals
- C21D 1/26: Methods of annealing
- C21D 6/00: Heat treatment of ferrous alloys
- C21D 6/004: {containing Cr and Ni}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0263: {following hot rolling}
- C21D 8/0273: {Final recrystallisation annealing}
- C22C 38/00: Ferrous alloys, e.g. steel alloys (cast-iron alloys C22C37/00)
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/004: {Very low carbon steels, i.e. having a carbon content of less than 0,01%}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/008: {containing tin}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/42: with copper
- C22C 38/44: with molybdenum or tungsten
- C22C 38/46: with vanadium
- C22C 38/48: with niobium or tantalum
- C22C 38/50: with titanium or zirconium
- C22C 38/52: with cobalt
- C22C 38/54: with boron
- C22C 38/60: containing lead, selenium, tellurium, or antimony, or more than 0.04% by weight of sulfur
- C21D 2211/005: Ferrite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

A ferritic stainless steel sheet has a predetermined chemical composition and thickness, and has an area ratio of crystal grains of 45 μm or more in grain size of 20% or less.

## Claims

### Claim 1

A ferritic stainless steel sheet comprising:
a chemical composition containing, in mass %,
C: 0.001% to 0.020%,
Si: 0.05% to 1.00%,
Mn: 0.05% to 1.50%,
P: 0.04% or less,
S: 0.010% or less,
Al: 0.001% to 0.300%,
Cr: 10.0% to 13.0%,
Ni: 0.65% to 1.50%,
Ti: 0.15% to 0.35%, and
N: 0.001% to 0.020%,
with a balance consisting of Fe and inevitable impurities;
an area ratio of crystal grains of 45 μm or more in grain size of 20% or less; and
a thickness of 5.0 mm or more.

### Claim 2 (depends on 1)

The ferritic stainless steel sheet according to claim 1, wherein the chemical composition further contains, in mass %, one or more selected from
Cu: 0.01% to 1.00%,
Mo: 0.01% to 1.00%,
W: 0.01% to 0.20%, and
Co: 0.01% to 0.20%.

### Claim 3 (depends on 1)

The ferritic stainless steel sheet according to claim 1, wherein the chemical composition further contains, in mass %, one or more selected from
V: 0.01% to 0.20%,
Nb: 0.01% to 0.10%, and
Zr: 0.01% to 0.20%.

### Claim 4 (depends on 1)

The ferritic stainless steel sheet according to claim 1, wherein the chemical composition further contains, in mass %, one or more selected from
B: 0.0002% to 0.0050%,
REM: 0.001% to 0.100%,
Mg: 0.0005% to 0.0030%,
Ca: 0.0003% to 0.0050%,
Sn: 0.001% to 0.500%, and
Sb: 0.001% to 0.500%.

### Claim 5 (depends on 1)

A method for producing the ferritic stainless steel sheet according to claim 1, the method comprising the following (a) and (b) and optionally comprising the following (c):
(a) heating a slab having the chemical composition according to claim 1 to a temperature range of 1050° C. or more and 1250° C. or less;
(b) subjecting the slab to hot rolling at a cumulative rolling reduction in a temperature range of T1 [° C.] to T2 [° C.] of 50% or more and a coiling temperature of 500° C. or more, to obtain a hot-rolled steel sheet; and
(c) subjecting the hot-rolled steel sheet to hot-rolled sheet annealing in a temperature range of 600° C. or more and less than 800° C.,
wherein T1 and T2 are respectively defined by the following formulas (1) and (2):
T1[° C.]=144Ni+66Mn+885 (1)
T2[° C.]=91Ni+40Mn+1083 (2)
where Ni and Mn are respectively Ni content and Mn content in mass % in the chemical composition of the slab.

### Claim 6 (depends on 2)

The ferritic stainless steel sheet according to claim 2, wherein the chemical composition further contains, in mass %, one or more selected from
V: 0.01% to 0.20%,
Nb: 0.01% to 0.10%, and
Zr: 0.01% to 0.20%.

### Claim 7 (depends on 2)

The ferritic stainless steel sheet according to claim 2, wherein the chemical composition further contains, in mass %, one or more selected from
B: 0.0002% to 0.0050%,
REM: 0.001% to 0.100%,
Mg: 0.0005% to 0.0030%,
Ca: 0.0003% to 0.0050%,
Sn: 0.001% to 0.500%, and
Sb: 0.001% to 0.500%.

### Claim 8 (depends on 3)

The ferritic stainless steel sheet according to claim 3, wherein the chemical composition further contains, in mass %, one or more selected from
B: 0.0002% to 0.0050%,
REM: 0.001% to 0.100%,
Mg: 0.0005% to 0.0030%,
Ca: 0.0003% to 0.0050%,
Sn: 0.001% to 0.500%, and
Sb: 0.001% to 0.500%.

### Claim 9 (depends on 6)

The ferritic stainless steel sheet according to claim 6, wherein the chemical composition further contains, in mass %, one or more selected from
B: 0.0002% to 0.0050%,
REM: 0.001% to 0.100%,
Mg: 0.0005% to 0.0030%,
Ca: 0.0003% to 0.0050%,
Sn: 0.001% to 0.500%, and
Sb: 0.001% to 0.500%.

### Claim 10 (depends on 2)

A method for producing the ferritic stainless steel sheet according to claim 2, the method comprising the following (a) and (b) and optionally comprising the following (c):
(a) heating a slab having the chemical composition according to claim 2 to a temperature range of 1050° C. or more and 1250° C. or less;
(b) subjecting the slab to hot rolling at a cumulative rolling reduction in a temperature range of T1 [° C.] to T2 [° C.] of 50% or more and a coiling temperature of 500° C. or more, to obtain a hot-rolled steel sheet; and
(c) subjecting the hot-rolled steel sheet to hot-rolled sheet annealing in a temperature range of 600° C. or more and less than 800° C.,
wherein T1 and T2 are respectively defined by the following formulas (1) and (2):
T1[° C.]=144Ni+66Mn+885 (1)
T2[° C.]=91Ni+40Mn+1083 (2)
where Ni and Mn are respectively Ni content and Mn content in mass % in the chemical composition of the slab.

### Claim 11 (depends on 3)

A method for producing the ferritic stainless steel sheet according to claim 3, the method comprising the following (a) and (b) and optionally comprising the following (c):
(a) heating a slab having the chemical composition according to claim 3 to a temperature range of 1050° C. or more and 1250° C. or less;
(b) subjecting the slab to hot rolling at a cumulative rolling reduction in a temperature range of T1 [° C.] to T2 [° C.] of 50% or more and a coiling temperature of 500° C. or more, to obtain a hot-rolled steel sheet; and
(c) subjecting the hot-rolled steel sheet to hot-rolled sheet annealing in a temperature range of 600° C. or more and less than 800° C.,
wherein T1 and T2 are respectively defined by the following formulas (1) and (2):
T1[° C.]=144Ni+66Mn+885 (1)
T2[° C.]=91Ni+40Mn+1083 (2)
where Ni and Mn are respectively Ni content and Mn content in mass % in the chemical composition of the slab.

### Claim 12 (depends on 4)

A method for producing the ferritic stainless steel sheet according to claim 4, the method comprising the following (a) and (b) and optionally comprising the following (c):
(a) heating a slab having the chemical composition according to claim 4 to a temperature range of 1050° C. or more and 1250° C. or less;
(b) subjecting the slab to hot rolling at a cumulative rolling reduction in a temperature range of T1 [° C.] to T2 [° C.] of 50% or more and a coiling temperature of 500° C. or more, to obtain a hot-rolled steel sheet; and
(c) subjecting the hot-rolled steel sheet to hot-rolled sheet annealing in a temperature range of 600° C. or more and less than 800° C.,
wherein T1 and T2 are respectively defined by the following formulas (1) and (2):
T1[° C.]=144Ni+66Mn+885 (1)
T2[° C.]=91Ni+40Mn+1083 (2)
where Ni and Mn are respectively Ni content and Mn content in mass % in the chemical composition of the slab.

### Claim 13 (depends on 6)

A method for producing the ferritic stainless steel sheet according to claim 6, the method comprising the following (a) and (b) and optionally comprising the following (c):
(a) heating a slab having the chemical composition according to claim 6 to a temperature range of 1050° C. or more and 1250° C. or less;
(b) subjecting the slab to hot rolling at a cumulative rolling reduction in a temperature range of T1 [° C.] to T2 [° C.] of 50% or more and a coiling temperature of 500° C. or more, to obtain a hot-rolled steel sheet; and
(c) subjecting the hot-rolled steel sheet to hot-rolled sheet annealing in a temperature range of 600° C. or more and less than 800° C.,
wherein T1 and T2 are respectively defined by the following formulas (1) and (2):
T1[° C.]=144Ni+66Mn+885 (1)
T2[° C.]=91Ni+40Mn+1083 (2)
where Ni and Mn are respectively Ni content and Mn content in mass % in the chemical composition of the slab.

### Claim 14 (depends on 7)

A method for producing the ferritic stainless steel sheet according to claim 7, the method comprising the following (a) and (b) and optionally comprising the following (c):
(a) heating a slab having the chemical composition according to claim 7 to a temperature range of 1050° C. or more and 1250° C. or less;
(b) subjecting the slab to hot rolling at a cumulative rolling reduction in a temperature range of T1 [° C.] to T2 [° C.] of 50% or more and a coiling temperature of 500° C. or more, to obtain a hot-rolled steel sheet; and
(c) subjecting the hot-rolled steel sheet to hot-rolled sheet annealing in a temperature range of 600° C. or more and less than 800° C.,
wherein T1 and T2 are respectively defined by the following formulas (1) and (2):
T1[° C.]=144Ni+66Mn+885 (1)
T2[° C.]=91Ni+40Mn+1083 (2)
where Ni and Mn are respectively Ni content and Mn content in mass % in the chemical composition of the slab.

### Claim 15 (depends on 8)

A method for producing the ferritic stainless steel sheet according to claim 8, the method comprising the following (a) and (b) and optionally comprising the following (c):
(a) heating a slab having the chemical composition according to claim 8 to a temperature range of 1050° C. or more and 1250° C. or less;
(b) subjecting the slab to hot rolling at a cumulative rolling reduction in a temperature range of T1 [° C.] to T2 [° C.] of 50% or more and a coiling temperature of 500° C. or more, to obtain a hot-rolled steel sheet; and
(c) subjecting the hot-rolled steel sheet to hot-rolled sheet annealing in a temperature range of 600° C. or more and less than 800° C.,
wherein T1 and T2 are respectively defined by the following formulas (1) and (2):
T1[° C.]=144Ni+66Mn+885 (1)
T2[° C.]=91Ni+40Mn+1083 (2)
where Ni and Mn are respectively Ni content and Mn content in mass % in the chemical composition of the slab.

### Claim 16 (depends on 9)

A method for producing the ferritic stainless steel sheet according to claim 9, the method comprising the following (a) and (b) and optionally comprising the following (c):
(a) heating a slab having the chemical composition according to claim 9 to a temperature range of 1050° C. or more and 1250° C. or less;
(b) subjecting the slab to hot rolling at a cumulative rolling reduction in a temperature range of T1 [° C.] to T2 [° C.] of 50% or more and a coiling temperature of 500° C. or more, to obtain a hot-rolled steel sheet; and
(c) subjecting the hot-rolled steel sheet to hot-rolled sheet annealing in a temperature range of 600° C. or more and less than 800° C.,
wherein T1 and T2 are respectively defined by the following formulas (1) and (2):
T1[° C.]=144Ni+66Mn+885 (1)
T2[° C.]=91Ni+40Mn+1083 (2)