# US 2021/0343457 A1 · Permanent magnet, rotary electrical machine, and vehicle

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0343457 A1
- Document ID: US20210343457A1
- Status: Published application
- Kind: A1
- Application number: 17/375,064
- Filed: 2021-07-14
- Published: 2021-11-04
- Earliest claimed: 2017-09-15
- Assignees: Kabushiki Kaisha Toshiba
- Applicants: Kabushiki Kaisha Toshiba
- Inventors: Masaya Hagiwara; Yosuke Horiuchi; Shinya Sakurada
- Web page: https://patentgrep.com/patent/US20210343457A1

## CPC

- H01F 1/0557: {sintered}
- B22F 3/24: After-treatment of workpieces or articles {(B22F3/1146 takes precedence)}
- B22F 2003/248: {Thermal after-treatment}
- B22F 2998/10: Processes characterised by the sequence of their steps
- B22F 2999/00: Aspects linked to processes or compositions used in powder metallurgy
- C22C 19/07: based on cobalt
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/10: containing cobalt
- C22C 38/14: containing titanium or zirconium
- C22C 38/16: containing copper
- H01F 41/0266: {Moulding; Pressing (H01F41/0273 takes precedence; hard magnetic particles H01F1/06, H01F1/11)}
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES
- B22F: WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER (making alloys by powder metallurgy C22C); APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

A permanent magnet is expressed by a composition formula: RpFeqMrCu5Co100-p-q-r-s. The magnet includes a crystal grain having a main phase including a TbCu7 crystal phase, and a volume ratio of the TbCu7 crystal phase to the main phase is 95% or more.

## Claims

### Claim 1

A method of manufacturing a permanent magnet, comprising:
preparing an alloy powder, the alloy powder being expressed by a composition formula: RpFeqMrCusCo100-p-q-r-s
where R is at least one element selected from the group consisting of rare-earth elements, M is at least one element selected from the group consisting of Zr, Ti, and Hf, p is a number satisfying 10.5≤p≤12.5 atomic percent, q is a number satisfying 25≤q≤40 atomic percent, r is a number satisfying 0.88≤r≤4.5 atomic percent, and s is a number satisfying 3.5 ≤s≤10.7 atomic percent;
press-forming the alloy powder in a magnetic field to form a green compact;
sintering the green compact to form a sintered compact;
performing a solution heat treatment on the sintered compact at a temperature of not less than 1100° C. nor more than 1180° C.; and
performing an aging treatment on the compact after the solution heat treatment, the aging treatment including
heating the compact at a temperature of not lower than 550° C. nor higher than 680° C. for not less than 1 hour nor more than 100 hours, and then
cooling the compact at a cooling rate of not less than 0.1° C./minute nor more than 5° C./minute to a temperature of not lower than 20° C. nor higher than 500° C.

### Claim 2 (depends on 1)

The method according to claim 1,
wherein the magnet comprises a crystal grain having a main phase, the main phase including a TbCu7 crystal phase,
wherein a volume ratio of the TbCu7 crystal phase to the main phase is 95% or more,
wherein the TbCu7 crystal phase has a variation in Cu concentration, and
wherein a variance of the Cu concentration in the TbCu7 crystal phase is 0.7 or more.

### Claim 3 (depends on 1)

The method according to claim 1,
wherein the magnet gives an X-ray diffraction pattern having a relative intensity of a peak ascribed to a Th2Zn17 crystal phase at a diffraction angle 2θ of 37.5 degree or more and 38.5 degree or less to a maximum peak ascribed to the TbCu7 crystal phase, the relative intensity being 0.4 or less.

### Claim 4 (depends on 1)

The method according to claim 1,
wherein the green compact is sintered at a temperature of not lower than 1180° C. nor higher than 1250° C. for not less than 0.5 hours nor more than 15 hours.

### Claim 5 (depends on 1)

The method according to claim 1, further comprising performing a rapid cooling on the compact after the solution heat treatment before the aging treatment at a cooling rate of less than 150° C./minute to a room temperature.

### Claim 6 (depends on 1)

The method according to claim 1,
wherein the alloy powder is prepared by pulverizing an alloy ingot made of a casting and expressed by the composition formula, the alloy powder having an average particle size of not less than 2 μm nor more than 8 μm.

### Claim 7 (depends on 1)

The method according to claim 1,
wherein the magnet comprises a crystal grain having a main phase, the main phase including a TbCu7 crystal phase,
wherein a volume ratio of the TbCu7 crystal phase to the main phase is 95% or more, wherein the TbCu7 crystal phase has a variation in Cu concentration, wherein a variance of the Cu concentration in the TbCu7 crystal phase is 0.7 or more, and
wherein the magnet gives an X-ray diffraction pattern having a relative intensity of a peak ascribed to a Th2Zn17 crystal phase at a diffraction angle 2θ of 37.5 degree or more and

### Claim 8 (depends on 1)

The method according to claim 1,
wherein the green compact is sintered at a temperature of not lower than 1180° C. nor higher than 1250° C. for not less than 0.5 hours nor more than 15 hours, wherein the magnet comprises a crystal grain having a main phase, the main phase including a TbCu7 crystal phase,
wherein a volume ratio of the TbCu7 crystal phase to the main phase is 95% or more, wherein the TbCu7 crystal phase has a variation in Cu concentration, wherein a variance of the Cu concentration in the TbCu7 crystal phase is 0.7 or more, and
wherein the magnet gives an X-ray diffraction pattern having a relative intensity of a peak ascribed to a Th2Zn17 crystal phase at a diffraction angle 2θ of 37.5 degree or more and 38.5 degree or less to a maximum peak ascribed to the TbCu7 crystal phase, the relative intensity being 0.4 or less.

### Claim 38

5 degree or less to a maximum peak ascribed to the TbCu7 crystal phase, the relative intensity being 0.4 or less.