# US 2021/0343456 A1 · Sintered r2m17 magnet and method of fabricating a r2m17 magnet

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0343456 A1
- Document ID: US20210343456A1
- Status: Published application
- Kind: A1
- Application number: 16/865,982
- Filed: 2020-05-04
- Published: 2021-11-04
- Earliest claimed: 2020-05-04
- Assignees: Vacuumschmelze GmbH & Co. KG
- Applicants: Vacuumschmelze GmbH & Co. KG
- Inventors: Kaan ÜSTÜNER; Matthias KATTER; Christoph BROMBACHER
- Web page: https://patentgrep.com/patent/US20210343456A1

## CPC

- H01F 1/0557: {sintered}
- H01F 1/0536: {sintered}
- H01F 7/0205: {Magnetic circuits with PM in general}
- H01F 41/0273: {Imparting anisotropy (methods and devices for magnetising permanent magnets H01F13/003)}
- H01F 41/22: Heat treatment; Thermal decomposition; Chemical vapour deposition
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES

## Abstract

A sintered R2M17 magnet is provided that comprises at least 70 Vol % of a Sm2M17 phase, wherein R is at least one of the group consisting of Ce, La, Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yt, Lu and Y, and M comprises Co, Fe, Cu and Zr. In an area of the R2M17 sintered magnet of 200 by 200 μm viewed in a Kerr micrograph, an areal proportion of demagnetised regions after application of an internal opposing field of 1200 kA/m is less than 5% or less than 2%.

## Claims

### Claim 1

A method of fabricating a R2M17 alloy magnet, wherein R is at least one of the group consisting of Ce, La, Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu and Y and M comprises Co, Fe, Cu and Zr, wherein the R2M17 alloy comprises a phase diagram that comprises with decreasing temperature a first phase field, a second phase field and a third phase field, the phase diagram comprising a first boundary between the first phase field and the second phase field, the first phase field comprising a liquid phase and a solid R2M17 phase in equilibrium and the second phase field comprising a solid R2M17 majority phase with a phase fraction of larger than 95%, and a second boundary between the second phase field and the third phase field, the third phase field comprising a solid R2M17 phase and at least one further solid phase of differing composition in equilibrium, the method comprising:
heat treating a body comprising a ratio of 2R and 17M, wherein R is at least one of the group consisting of Ce, La, Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu and Y, and M comprises Co, Fe, Cu and Zr, at a first temperature TS above the first boundary and in the first phase field, followed by
cooling the body through the first boundary followed by
heating up the body through the first boundary and heat treating the body at a temperature TAH between the first boundary and the first temperature TS, followed by
cooling the body through the first boundary and heat treating the body at a temperature below the first boundary.

### Claim 2 (depends on 1)

The method of claim 1, further comprising repeating:
the heating up the body through the first boundary and heat treating the body at a temperature TAH between the first boundary and the first temperature TS, followed by the cooling of the body through the first boundary and heat treating the body at a temperature below the first boundary.

### Claim 3

A method of fabricating a R2M17 alloy magnet, wherein R is at least one of the group consisting of Ce, La, Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu and Y, and M comprises Co, Fe, Cu and Zr, wherein the R2M17 alloy comprises a phase diagram that comprises with decreasing temperature a first phase field, a second phase field and a third phase field, the phase diagram comprising a first boundary between the first phase field and the second phase field, the first phase field comprising a liquid phase and a solid R2M17 phase in equilibrium and the second phase field comprising a solid R2M17 majority phase with a phase fraction of larger than 95%, and a second boundary between the second phase field and the third phase field, the third phase field comprising a solid R2M17 phase and at least one further solid phase of differing composition in equilibrium, the method comprising:
heat treating a body comprising a ratio of 2R and 17M, wherein R is at least one of the group consisting of Ce, La, Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu and Y, and M comprises Co, Fe, Cu and Zr, at a first temperature TS above the first boundary and in the first phase field, followed by
cooling the body through the first boundary, followed by
cooling the body through the second boundary and heat treating the body at a temperature TBH below the second boundary and above 900° C., followed by
heating up the body through the second boundary and heat treating the body at a temperature between the second boundary and the first temperature TS.

### Claim 4 (depends on 3)

The method of claim 3, further comprising repeating:
the cooling the body through the second boundary and heat treating the body at a temperature TBH below the second boundary and above 900° C., followed by
the heating up the body through the second boundary and heat treating the body at a temperature between the second boundary and the first temperature TS.

### Claim 5 (depends on 1)

The method of claim 1, further comprising, after cooling the body through the first boundary, heat treating the body at a temperature TH between the first boundary and the second boundary.

### Claim 6 (depends on 1)

The method of claim 1, wherein a heat treatment dwell time at at least one of the temperatures, TS; TH; TAH and TBH is 30 min to 4 h.

### Claim 7 (depends on 1)

The method of claim 1, further comprising a final heat treatment at a temperature THf that is below the first boundary and above the second boundary and comprises a dwell time at THf of 2 to 16 h.

### Claim 8 (depends on 1)

The method of claim 1, wherein a cooling rate or a heating rate from one heat treatment step to the next heat treatment step is 0.2 to 5 K/min

### Claim 9 (depends on 1)

The method of claim 1, wherein the body is cooled through the second boundary to a temperature of less than 950° C. at a cooling rate of greater than 10K/min.

### Claim 10 (depends on 9)

The method of claim 9, further comprising, after the body is cooled through the second boundary, carrying out a last stage heat treatment only once, the last stage heat treatment comprising:
heat treating the body at a temperature of 800° C. to 950° C. for 2 hours to 60 hours, followed by
cooling to 500° C. at a cooling rate of less than 2K/min and heat treating at 300° C. to 500° C. for 0.5 hours to 6 hours.

### Claim 11 (depends on 5)

The method of claim 5, wherein TH is 5° C. to 40° C. less than TS.

### Claim 12 (depends on 11)

The method of claim 11, wherein TS lies in the range of 1155° C. to 1210° C., TH lies in the range of 1120° C. to 1170° C. and TAH lies in the range of 1135° C. to 1200° C.

### Claim 13 (depends on 1)

The method of claim 1, wherein M further comprises at least one of the group consisting of Ni, Hf and Ti.

### Claim 14 (depends on 13)

The method according to claim 13, wherein the R2M17 alloy comprises 0 wt %≤Hf≤3 wt %, 0 wt %≤Ti≤3 wt % and 0 wt %≤Ni≤10 wt %.

### Claim 15 (depends on 1)

The method of claim 1, wherein the R2M17 alloy comprises 23 wt % to 27 wt % Sm, 14 wt % to 25 wt % Fe, 39 wt % to 57 wt % Co, 4 wt % to 6 wt % Cu, 2 wt % to 3 wt % Zr, maximum 0.06 wt % C, maximum 0.4 wt % O and maximum 0.06 wt % N.

### Claim 16 (depends on 1)

The method of claim 1, wherein the R2M17 alloy is milled to a powder with an average particle size D50 of 4 μm to 8 μm, the powder is aligned in a magnetic field and pressed to a green part which is sintered to a magnet and the sintered magnet has an average grain size of at least 50 μm.

### Claim 17

A sintered R2M17 magnet, comprising:
at least 70 Vol % of a R2M17 phase, wherein R is at least one of the group consisting of Ce, La, Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yt, Lu and Y, and M comprises Co, Fe, Cu and Zr,
wherein, in an area of the R2M17 sintered magnet of ≥200 by 200 μm viewed in a Kerr micrograph, an areal proportion of demagnetised regions after application of an internal opposing field of 1200 kA/m is less than 5% or less than 2%.

### Claim 18 (depends on 17)

The sintered R2M17 magnet of claim 17, further comprising an average grain size of >50 μm.

### Claim 19 (depends on 17)

The sintered R2M17 magnet of claim 17, further comprising a coercive field strength HcB of greater than 840 kA/m or greater than 860 kA/m.

### Claim 20 (depends on 17)

The sintered R2M17 magnet of claim 17, further comprising a reversible permeability of less than 1.10 or 1.08.

### Claim 21 (depends on 17)

The sintered R2M17 magnet of claim 17, wherein M further comprises at least one of the group consisting of Ni, Hf and Ti.

### Claim 22 (depends on 21)

The sintered R2M17 magnet according to claim 21, wherein 0 wt %≤Hf≤3 wt %, 0 wt %≤Ti≤3 wt % and 0 wt %≤Ni≤10 wt %.

### Claim 23 (depends on 17)

The sintered R2M17 magnet of claim 17, wherein the sintered R2M17 magnet comprises 23 wt % to 27 wt % Sm, 14 wt % to 25 wt % Fe, 39 wt % to 57 wt % Co, 4 wt % to 6 wt % Cu, 2 wt % to 3 wt % Zr, maximum 0.06 wt % C, maximum 0.4 wt % O and maximum 0.06 wt % N.