# US 2021/0340654 A1 · Method of making 6xxx aluminium sheets with high surface quality

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0340654 A1
- Document ID: US20210340654A1
- Status: Published application
- Kind: A1
- Application number: 17/298,387
- Filed: 2019-12-04
- Published: 2021-11-04
- Earliest claimed: 2018-12-11
- Assignees: Constellium Neuf-Brisach
- Applicants: Constellium Neuf-Brisach
- Inventors: Estelle MULLER; Gilles GUIGLIONDA; Philipp LABOISSIERE; Laurent FERRY
- Web page: https://patentgrep.com/patent/US20210340654A1

## CPC

- C22F 1/043: of alloys with silicon as the next major constituent
- C22F 1/05: of alloys of the Al-Si-Mg type, i.e. containing silicon and magnesium in approximately equal proportions
- C22C 21/02: with silicon as the next major constituent
- C22C 21/08: with silicon
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

The invention is directed to a method for producing a 6xxx series aluminium sheet comprising the steps of homogenizing an ingot made from a 6XXX series aluminium alloy comprising in wt. % Si: 0.4-0.7, Mg: 0.2-0.4, Mn: 0.05-0.30, Fe: 0.03 to 0.4, Cu up to 0.3, Cr up to 0.05, Zn up to 0.15, Ti up to 0.1 wt %, rest aluminium and unavoidable impurities up to 0.05 each and 0.15 total, rough hot rolling on a reversible mill to a rough hot rolling exit thickness with a rough hot rolling exit temperature less than 420° C., finish hot rolling the ingot to a hot rolling final thickness with a tandem mill and coiling at the hot rolling final thickness with a hot rolling exit temperature less than 300° C., cold rolling to obtain a cold rolled sheet. The products obtained according to the method of the invention are particularly useful for automobile hood inners as they have the requested mechanical properties for pedestrian safety and surface quality.

## Claims

### Claim 1

A method for producing a 6xxx series aluminum sheet comprising
homogenizing an ingot made from a 6XXX series aluminum alloy comprising in wt. %
Si: 0.4-0.7,
Mg: 0.2-0.4,
Mn: 0.05-0.30,
Fe: 0.03 to 0.4,
Cu up to 0.3,
Cr up to 0.05,
Zn up to 0.15,
Ti up to 0.1 wt %,
rest aluminum and unavoidable impurities up to 0.05 each and 0.15 total,
rough hot rolling on a reversible mill to a rough hot rolling exit thickness with a rough hot rolling exit temperature less than 420° C.,
finish hot rolling the ingot to a hot rolling final thickness with a tandem mill and coiling at the hot rolling final thickness with a hot rolling exit temperature less than 300° C.,
cold rolling to obtain a cold rolled sheet.

### Claim 2 (depends on 1)

The method according to claim 1 wherein Cu content is from 0.08 to 0.15 wt. % and/or the Si content is from 0.55 to 0.65 wt. %.

### Claim 3 (depends on 1)

The method according to claim 1 wherein the hot rolled sheet obtained after finish hot rolling exhibits at most 50% recrystallization rate.

### Claim 4 (depends on 1)

The method according to claim 1 wherein the homogenized ingot is cooled with a cooling rate in a range from 150° C./h to 2000° C./h directly to a hot rolling starting temperature, between 370° C. and 430° C.

### Claim 5 (depends on 1)

The method according to claim 1 wherein the ingot thickness is at least 250 mm and wherein optionally the ingot is from 1000 to 2000 mm in width and 2000 to 8000 mm in length and wherein a thermal differential of less than 40° C. over the entire ingot cooled from the homogenization temperature is obtained at the hot rolling starting temperature.

### Claim 6 (depends on 1)

The method according to claim 1 wherein the cold rolled sheet is further solution heat treated and quenched in a continuous annealing line.

### Claim 7 (depends on 6)

The method according to claim 6 wherein the continuous annealing line is operated in such a way that a temperature of at least 460° C., optionally at least 500° C., or 520° C. or even 530° C. is reached by the sheet, optionally between 540° C. and 560° C.

### Claim 8 (depends on 6)

The method according to claim 6 wherein the coiling temperature after solution heat treatment is up to 85° C., optionally up to 65° C. and optionally between 45° C. and 65° C.

### Claim 9 (depends on 6)

The method according to claim 6 wherein after solution heat treatment and quench the sheet is aged to a T4 temper, cut and formed to final shape, painted and bake hardened.

### Claim 10 (depends on 6)

The 6xxx series aluminum sheet obtainable by the method of claim 6 having a roping value “RK” according to VDA Recommendation 239-400 of less than 5 and a TYS in the LT direction after bake hardening, TYS(LT)BH between 90 MPa and 150 MPa.

### Claim 11 (depends on 10)

The sheet according to claim 10 having a Si content between 0.55 wt. % and 0.60 wt. % a Mg content is 0.25 wt. % and 0.30 wt. %, a roping value “RK” according to VDA Recommendation 239-400 of less than 5.0 and optionally of less than 4.0 and a TYS in the LT direction after bake hardening obtained by 2% stretching and 20 min at 185° C., referred to as TYS(LT)BH, between 90 MPa and 120 MPa.

### Claim 12 (depends on 10)

The sheet according to claim 10 having a Si content between 0.60 wt. % and 0.65 wt. %, a Mg content between 0.30 wt. % and 0.35 wt. %, a roping value “RK” according to VDA Recommendation 239-400 of less than 5.0 and a TYS in the LT direction after bake hardening obtained by 2% stretching and 20 min at 185° C., referred to as TYS(LT)BH, between 120 MPa and 150 MPa.

### Claim 13 (depends on 10)

A product comprising a 6xxx series aluminum sheet according to claim 10 as an automobile hood inner.