# US 2021/0332186 A1 · Polymer film, method of preparing the same, and flexible folding panel

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0332186 A1
- Document ID: US20210332186A1
- Status: Published application
- Kind: A1
- Application number: 16/624,149
- Filed: 2019-11-04
- Published: 2021-10-28
- Earliest claimed: 2019-08-19
- Assignees: Wuhan China Star Optoelectronics Semiconductor Display Technology Co., Ltd.
- Applicants: Wuhan China Star Optoelectronics Semiconductor Display Technology Co., Ltd.
- Inventors: Yuan ZHAO
- Web page: https://patentgrep.com/patent/US20210332186A1

## CPC

- C08G 18/341: {Dicarboxylic acids, esters of polycarboxylic acids containing two carboxylic acid groups}
- C08J 7/0427: {with only one layer of a composition containing a polymer binder (with more layers C08J7/042)}
- C08G 18/7671: {containing only one alkylene bisphenyl group}
- C08G 18/7678: {containing condensed aromatic rings}
- C08G 18/78: Nitrogen {(C08G18/775, C08G18/776 take precedence)}
- C08J 5/18: Manufacture of films or sheets
- C08J 7/046: Forming abrasion-resistant coatings; Forming surface-hardening coatings
- C09D 175/04: Polyurethanes
- C08J 2379/08: Polyimides; Polyester-imides; Polyamide-imides; Polyamide acids or similar polyimide precursors
- C08J 2475/04: Polyurethanes
- G09F 9/301: {flexible foldable or roll-able electronic displays, e.g. thin LCD, OLED}
- C08G: MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
- C08J: WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H (working, e.g. shaping, of plastics B29)
- C09D: COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR (cosmetics A61K; processes for applying liquids or other fluent materials to surfaces, in general, B05D; staining wood B27K5/02; glazes or vitreous enamels C03C; natural resins, French polish, drying-oils, driers, turpentine, per se, C09F; polishing compositions other than French polish, ski waxes C09G; adhesives or use of materials as adhesives C09J; materials for sealing or packing joints or covers C09K3/10; materials for stopping leaks C09K3/12; processes for the electrolytic or electrophoretic production of coatings C25D)
- G09F: DISPLAYING; ADVERTISING; SIGNS; LABELS OR NAME-PLATES; SEALS

## Abstract

The present disclosure provides a polymer film, a method of preparing the same, and a flexible folded panel. The polymer film includes a substrate and a strengthening layer, wherein the strengthening layer includes a polymer, side chains of the polymer include a plurality of rigid segments and a plurality of flexible segments, which modify and strengthen the side chains of the polymer. The monomer of the polymer is subjected to a series of reactions, to synthesize the polymer, and the polymer film enhance hardness of a cover plate of a panel and improve the anti-friction properties and bendability.

## Claims

### Claim 1

A method of preparing a polymer film, comprising the following steps:
S100: mixing bis(3-bromo-4-isocyanatophenyl)methane with an additive for reaction to prepare a monomer;
S101: reacting the monomer with oxalic acid to prepare a polymer; and
S102: coating the polymer on a substrate to form the polymer film,
wherein the monomer comprises: N,N′-(methylenebis(6-isocyanato-3,1-phenylene))bis(4-hexylnaphthalen-1-amine) or N,N′-(methylene bis(6-isocyanato-3,1-phenyiene)) bis(10-octylanthracene-9-amine); and
the polymer has a chemical structural formula as follows:
wherein n is a positive integer.

### Claim 2 (depends on 1)

The method of preparing the polymer film according to claim 1, wherein the additive comprises 4-hexylnaphthylamine.

### Claim 3 (depends on 1)

The method of preparing the polymer film according to claim 1, wherein the step S100 further comprises the following steps:
S200: adding the bis(3-bromo-4-isocyanatophenyl)methane and 4-hexylnaphthylamine to a flask, and adding cesium carbonate, cuprous iodide and 18-crown-6 to the flask;
S201: introducing argon gas into the flask, and adding deoxygenated N,N′-dimethylpropylene urea to the flask to form a mixture, and reacting the mixture at 180° C. for 24 hours; and
S202: cooling the flask to room temperature, adding ice water to the flask, followed by extraction three times with dichloromethane, then combining organic extracts, after that, adding silica gel to the organic extracts, removing solvent from the organic extracts, and carrying out column chromatography to obtain the monomer.

### Claim 4 (depends on 3)

The method of preparing the polymer film according to claim 3, wherein the step S201 further comprises the following steps:
S300: mixing the N,N′-(methylenebis(6-isocyanato-3,1-phenylene)) bis(4-hexylnaphthalen-1-amine) and the oxalic acid in the flask for reaction at 80° C. for 12 hours;
S301: precipitating the mixture with methanol to obtain a white solid, and then extracting the white solid in n-hexane and acetone for two days to obtain the polymer.

### Claim 5 (depends on 4)

The method of preparing the polymer film according to claim 4, wherein the step S300 comprises: introducing argon gas into the flask and adding diluted hydrochloric acid to the flask.

### Claim 6 (depends on 1)

The method of preparing the polymer film according to claim 1, wherein the additive comprises 10-amino-9-octylanthracene.

### Claim 7 (depends on 1)

The method of preparing the polymer film according to claim 1, wherein the step S100 further comprises the following steps:
S400: adding the bis(3-bromo-4-isocyanatophenyl)methane and 10-amino-9-octylanthracene to a flask;
S401: introducing argon gas into the flask, and adding deoxygenated N,N′-dimethylpropylene urea to the flask to form a mixture, and reacting the mixture at 180° C. for 24 hours; and
S402: cooling the flask to room temperature, adding ice water to the flask, followed by extraction three times with dichloromethane, then combining organic extracts, after that, adding silica gel to the flask, removing solvent from the organic extracts, and carrying out column chromatography to obtain the polymer monomer.

### Claim 8 (depends on 7)

The method of preparing the polymer film according to claim 7, wherein the step S400 further comprises: adding cerium carbonate, cuprous iodide and 18-crown-6 to the flask.

### Claim 9 (depends on 3)

The method of preparing the polymer film according to claim 3, wherein the step S201 further comprises the following steps:
S500: mixing the N,N′-(methylenebis(6-isocyanato-3,1-phenylene)) bis(10-octylfluorene-9-amine) and the oxalic acid in a flask, and introducing argon gas and diluted hydrochloric acid for a reaction at 80° C. for 12 hours to obtain a mixture; and
S501: precipitating the mixture with methanol to obtain a white solid, and then extracting the white solid in n-hexane and acetone for two days to obtain the polymer.

### Claim 10

A polymer film comprising:
a substrate; and
a strengthening layer;
wherein the strengthening layer is disposed on the substrate, the strengthening layer comprises a polymer, and side chains of the polymer comprise a plurality of rigid segments and a plurality of flexible segments, wherein the side chains of the polymer are modified and strengthened by the rigid segments and the flexible segments.

### Claim 11 (depends on 10)

The polymer film according to claim 10, wherein the polymer has a chemical structural formula as follows:
wherein n is a positive integer.

### Claim 12 (depends on 10)

The polymer film according to claim 10, wherein the polymer has a chemical structural formula as follows:
wherein n is a positive integer.

### Claim 13

A method of preparing a polymer film, comprising, the following steps:
S100: mixing bis(3-bromo-4-isocyanatophenyl)methane with an additive for reaction to prepare a monomer;
S101: reacting the monomer with oxalic acid to prepare a polymer; and
S102: coating the polymer on a substrate to form the polymer film.

### Claim 14 (depends on 13)

The method of preparing the polymer film according to claim 13, wherein the monomer comprises: N,N′-(methylenebis(6-isocyanato-3, 1-phenylene))bis(4-hexylnaphthalen-1-amine) or N,N′-methylenebis(6-isocyanato-3,1-phenylene)) bis(10-octylanthracene-9-amine).

### Claim 15 (depends on 13)

The method of preparing the polymer film according to claim 13, wherein the additive comprises 4-hexylnaphthylamine, and the step S100 further comprises the following steps:
S200: adding bis(3-bromo-4-isocyanatophenyl)methane and 4-hexylnaphthylamine to a flask, and adding cesium carbonate, cuprous iodide and 18-crown-6 to the flask;
S201: introducing argon gas into the flask, and adding deoxygenated N,N′-dimethylpropylene urea to the flask to form a mixture, and reacting the mixture at 180° C. for 24 hours; and
S202: cooling the flask to room temperature, adding ice water to the flask, followed by extraction three times with dichloromethane, then combining organic extracts, after that, adding silica gel to the organic extracts, removing solvent from the organic extracts, and carrying out column chromatography to obtain the polymer monomer.

### Claim 16 (depends on 15)

The method of preparing the polymer film according to claim 15, wherein the step S201 further comprises the following steps:
S300: mixing the N,N′-(methylenebis(6-isocyanato-3,1-phenylene)) bis(4-hexylnaphthalen-1-amine) and the oxalic acid in the flask for reaction at 80° C for 12 hours; and
S301: precipitating the mixture with methanol to obtain a white solid, and then extracting the white solid in n-hexane and acetone for two days to obtain the polymer.

### Claim 17 (depends on 13)

The method of preparing the polymer film according to claim 13, wherein the additive comprises 10-amino-9-octylanthracene, and the step S100 further comprises the following steps:
S400: adding bis(3-bromo-4-isocyanatophenyl)methane and 10-amino-9-octylanthracene to a flask;
S401: introducing argon gas into the flask, and adding deoxygenated N,N′-dimethylpropylene urea to the flask to form a mixture, and reacting the mixture at 180° C. for 24 hours; and
S402: cooling the flask to room temperature, adding ice water to the flask, followed by extraction three times with dichloromethane, then combining organic extracts, after that, adding silica gel to the organic extracts, removing solvent from the organic extracts, and carrying out column chromatography to obtain the polymer monomer.

### Claim 18 (depends on 15)

The method of preparing the polymer film according to claim 15, wherein the step S201 further comprises the following steps:
S500: mixing the N,N′-(methylenebis(6-isocyanato-3,1-phenylene)) bis(10-octylfluorene-9-amine) and the oxalic acid in a flask, and introducing argon gas and diluted hydrochloric acid for reaction at 80° C. for 12 hours to obtain a mixture; and
S501: precipitating the mixture with methanol to obtain a white solid, and then extracting the white solid in n-hexane and acetone for two days to obtain the polymer.