# US 2021/0331932 A1 · Preparation and application of 4-methyl-5-vinylthiazolyl polymeric ionic liquid

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0331932 A1
- Document ID: US20210331932A1
- Status: Published application
- Kind: A1
- Application number: 16/613,193
- Filed: 2018-12-27
- Published: 2021-10-28
- Earliest claimed: 2018-11-14
- Assignees: Fu Zhou University
- Applicants: Fu Zhou University
- Inventors: Yuanyuan YUE; Ben LIU; Nangui LV; Xiaojun BAO; Jie LIU; Tinhai WANG; Pei YUAN; Haibo ZHU; Zhengshuai BAI; Qingyan CUI
- Web page: https://patentgrep.com/patent/US20210331932A1

## CPC

- C01B 39/40: using at least one organic template directing agent
- B01J 6/001: {Calcining}
- B01J 20/18: Synthetic zeolitic molecular sieves
- B01J 29/041: {Mesoporous materials having base exchange properties, e.g. Si/Al-MCM-41}
- B01J 29/042: {containing iron group metals, noble metals or copper}
- B01J 29/044: {Iron group metals or copper}
- B01J 29/46: Iron group metals or copper
- B01J 29/88: Ferrosilicates; Ferroaluminosilicates {(B01J29/005 takes precedence)}
- B01J 35/60: characterised by their surface properties or porosity
- B01J 35/647: {2-50 nm}
- B01J 37/04: Mixing {(B01J37/0009, B01J37/0018 take precedence)}
- B01J 37/06: Washing {(B01J37/0009, B01J37/0018 take precedence)}
- B01J 37/10: in the presence of water, e.g. steam
- F01N 3/0842: {Nitrogen oxides}
- F01N 3/2066: {Selective catalytic reduction [SCR]}
- B01D 2255/20738: Iron
- B01D 2255/20761: Copper
- B01D 2255/50: Zeolites
- B01D 2255/504: ZSM 5 zeolites
- B01D 2257/40: Nitrogen compounds
- B01D 2257/402: Dinitrogen oxide
- B01D 2257/404: Nitrogen oxides other than dinitrogen oxide
- B01D 2258/01: Engine exhaust gases
- B01D 2258/012: Diesel engines and lean burn gasoline engines
- B01J 2220/4806: the starting material being of inorganic character
- B01J 2229/183: in framework positions
- B01J 2229/186: not in framework positions
- B01J 2229/37: Acid treatment
- F01N 2370/04: Zeolitic material
- F01N 2570/14: Nitrogen oxides
- F01N 2570/145: Dinitrogen oxide
- Y02C 20/10: of nitrous oxide (N2O)
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}
- B01J: CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
- F01N: GAS-FLOW SILENCERS OR EXHAUST APPARATUS FOR MACHINES OR ENGINES IN GENERAL; GAS-FLOW SILENCERS OR EXHAUST APPARATUS FOR INTERNAL-COMBUSTION ENGINES (arrangements in connection with gas exhaust of propulsion units in vehicles B60K13/00; combustion-air intake silencers specially adapted for, or arranged on, internal-combustion engines F02M35/00; protecting against, or damping, noise in general G10K11/16)
- B01D: SEPARATION (separating solids from solids by wet methods B03B, B03D; by pneumatic jigs or tables B03B; by other dry methods B07; magnetic or electrostatic separation of solid materials from solid materials or fluids, separation by high-voltage electric fields B03C; centrifuges, vortex apparatus B04; presses per se for squeezing-out liquid from liquid-containing material B30B9/02; treatment of water C02F, e.g. softening by ion-exchange C02F1/42; {arrangements of air intake cleaners in gas turbine plants F02C7/05} ; arrangements or mounting of filters in air-conditioning, air-humidification or ventilation F24F13/28)
- Y02C: CAPTURE, STORAGE, SEQUESTRATION OR DISPOSAL OF GREENHOUSE GASES [GHG]

## Abstract

This invention belongs to the technical field of green preparation of environmentally friendly catalysts, and discloses a preparation method and application of mesoporous FeCu—ZSM-5 molecular sieve, in particular to a method for synthesizing mesoporous FeCu—ZSM-5 molecular sieve by one-pot method and the application in selective catalytic reduction (SCR) denitration reaction. This invention firstly proposes to combine the two calcinations after demolding and ion exchange into one, that is, the original powder is directly calcined to prepare a FeCu—ZSM-5 molecular sieve. The molecular sieve has several advantages such as window with wide temperature window, low cost, good hydrothermal stability and high SCR denitrification activity. Besides, the synthesis process does not use a (large) pore template, nor does it use a post-treatment method to construct the mesopores. Therefore, the method of the invention not only has the advantages of simple process, simple operation, but also good economic and environmental benefits.

## Claims

### Claim 1

A mesoporous FeCu—ZSM-5 molecular sieve, comprising: deionized water, aluminum source, silicon source, iron source, copper source, acid source and templating agents; the content of Fe2O3 in the molecular sieve is 0.1˜10% of the total weight of the molecular sieve, wherein the content of Fe in skeleton accounts for more than 95% of the total iron content, and is evenly distributed in the framework; the CuO content in the molecular sieve is 0.1˜10% of the total weight of the molecular sieve, wherein the content of Cu2+ accounts for more than 90% of the total copper content, and is evenly distributed on the inner surface of the molecular sieve.

### Claim 2

A process for producing mesoporous FeCu—ZSM-5 molecular sieve, comprising: a chemical reagent synthesis method or a mineral synthesis method.

### Claim 3 (depends on 2)

The process according to claim 2, wherein the chemical reagent synthesis method specifically includes the following steps:
(1) the deionized water, aluminum source, silicon source, iron source, copper source and templating agent are uniformly mixed under stirring conditions at 20-90° C., wherein the molar ratio of each substance in the synthetic system is SiO2/Al2O3=10˜∞, SiO2/Fe2O3=10˜350, SiO2/CuO=10˜150, Na2O/SiO2=0.1˜0.5, H2O/SiO2=10˜50, templating agent/SiO2=0.01˜0.5; after mixing, add the acid source to adjust the system pH to 5˜13 to carry out the first aging, then add the acid source again, adjust the system pH to 5˜13 to carry out the second aging, that is, obtain the aging gel,
(2) the aged gel obtained in the step (1) is transferred to a Teflon-lined reaction kettle for sealing crystallization, after crystallization, the product is cooled, filtered to remove the mother liquid, and the filter cake is washed with deionized water to neutrality, dried to obtain a solid, and then which the solid is passed through ion-exchange, filtered, washed, and dried to obtain a powder;
wherein the drying condition is 80-150° C., drying overnight;
(3) the powder obtained in the step (2) is placed in a muffle furnace and calcined to obtain a mesoporous FeCu—ZSM-5 molecular sieve.

### Claim 4 (depends on 3)

The process according to claim 3, wherein
the iron source is one or more of ferric nitrate, ferric chloride and ferric sulfate,
the copper source is one or more of copper nitrate, copper nitrate trihydrate, copper nitrate nonahydrate and copper chloride dihydrate,
the acid source is one or more of 2-Hydroxy-1,2,3-propanetricarboxylic acid, sulfurous acid, nitrous acid, sulfuric acid, hydrochloric acid, nitric acid, oxalic acid, acetic acid,
the silicon source is one or more of water glass, silica sol, tetraethyl orthosilicate, solid silica gel,
the aluminum source is one or more of sodium aluminate and aluminum sulfate,
the templating agent is tetraoctyl ammonium bromide, tetrabutylammonium bromide, CTMAB, tetrapropylammonium hydroxide, tetrapropylammonium bromide, hexylene glycol, butylamine, ethylamine.

### Claim 5 (depends on 2)

The process according to claim 2, wherein the mineral synthesis method specifically includes the following steps:
(1) mineral activation: aluminum source, silicon source, iron source and copper source are activated respectively;
(2) the activated mineral is mixed with sodium hydroxide, deionized water and seed crystals, wherein the molar ratio of each substance in the synthetic system is SiO2/Al2O3=10˜∞, SiO2/Fe2O3=10˜350, SiO2/CuO=10˜150, Na2O/SiO2=0.1˜0.5, H2O/SiO2=10˜50, templating agent/SiO2=0.01˜0.5; after mixing, add the acid source to adjust the system pH to 5˜13 to carry out aging, that is, obtain the aging gel,
(3) the aged gel obtained in the step (2) is transferred to a Teflon-lined reaction kettle for sealing crystallization, after crystallization, the product is cooled, filtered to remove the mother liquid, and the filter cake is washed with deionized water to neutrality, dried to obtain a solid, and then which the solid is passed through ion-exchange, filtered, washed, and dried to obtain a powder,
wherein the drying condition is 80-150° C., drying overnight;
(4) the powder obtained in the step (2) is placed in a muffle furnace and calcined to obtain a mesoporous FeCu—ZSM-5 molecular sieve.

### Claim 6 (depends on 5)

The process according to claim 5, wherein
the iron source is one or more of bauxite, diatomaceous earth, rectorite, pyrite, mica hematite, and red mud,
the copper source is one or more of magnetite, malachite, copper blue, and chalcopyrite,
the acid source is one or more of 2-Hydroxy-1,2,3-propanetricarboxylic acid, sulfurous acid, nitrous acid, sulfuric acid, hydrochloric acid, nitric acid, oxalic acid, acetic acid,
the silicon source is one or two of bauxite, diatomaceous earth, rectorite, natural zeolite or opal,
the aluminum source is one or more of mica, alumite, bauxite, diatomaceous earth, rectorite, natural zeolite,
the templating agent is tetraoctyl ammonium bromide, tetrabutylammonium bromide, CTMAB, tetrapropylammonium hydroxide, tetrapropylammonium bromide, hexylene glycol, butylamine, ethylamine.

### Claim 7 (depends on 3, 5)

The process according to claim 3 or claim 5, wherein aging is carried out at 60-90° C. for 2-12 h; the crystallization is carried out at 100-190° C. for 12-96 h.

### Claim 8 (depends on 3, 5)

The process according to claim 3 or claim 5, wherein the method for ion-exchange is as follows: mixing the dried solid with 0.1˜2 M NH4Cl solution according to a mass ratio of 1:10 to 1:30 for ion exchange, and heating and stirring at 10˜80° C. for 3˜8 h.

### Claim 9 (depends on 3, 5)

The process according to claim 3 or claim 5, wherein the calcination is carried out at 500˜600° C. for 4˜10 h.

### Claim 10 (depends on 1, 2, 3, 4, 5, 6, 7, 8, 9)

The application of mesoporous FeCu—ZSM-5 molecular sieve according to any of the claims 1-9 in the selective catalytic reduction of nitrogen oxides.