# US 2021/0331428 A1 · Fiber-reinforced resin molding material and method for manufacturing same, and fiber-reinforced resin molded article

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0331428 A1
- Document ID: US20210331428A1
- Status: Published application
- Kind: A1
- Application number: 17/368,889
- Filed: 2021-07-07
- Published: 2021-10-28
- Earliest claimed: 2017-04-25
- Assignees: Mitsubishi Chemical Corporation
- Applicants: Mitsubishi Chemical Corporation
- Inventors: Yukichi KONAMI
- Web page: https://patentgrep.com/patent/US20210331428A1

## CPC

- B29C 70/20: oriented in a single direction, e.g. roofing or other parallel fibres {(B29C70/083, B29C70/226 take precedence)}
- B29B 15/122: {with a matrix in liquid form, e.g. as melt, solution or latex}
- B29C 70/06: Fibrous reinforcements only
- B29C 70/22: oriented in at least two directions forming a two-dimensional [2D] structure
- B29K 2031/00: Use of polyvinylesters {or derivatives thereof} as moulding material
- B29K 2307/04: Carbon
- B29C: SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING (making preforms B29B11/00; making laminated products by combining previously unconnected layers which become one product whose layers will remain together B32B37/00 - B32B41/00)
- B29B: PREPARATION OR PRETREATMENT OF THE MATERIAL TO BE SHAPED; MAKING GRANULES OR PREFORMS; RECOVERY OF PLASTICS OR OTHER CONSTITUENTS OF WASTE MATERIAL CONTAINING PLASTICS
- B29K: INDEXING SCHEME ASSOCIATED WITH SUBCLASSES B29B, B29C OR B29D, RELATING TO MOULDING MATERIALS OR TO MATERIALS FOR {MOULDS, } REINFORCEMENTS, FILLERS OR PREFORMED PARTS, e.g. INSERTS

## Abstract

Provided are a fiber-reinforced resin molding material with which a lightweight and high-strength fiber-reinforced resin molded article can be easily obtained and a method for manufacturing the fiber-reinforced resin molding material. A fiber-reinforced resin molding material in which a reinforcement fiber sheet whose basis weight is 200 g/m2 or greater and 3,000 g/m2 or less is impregnated with a resin composition such that a content of the resin composition is 25 volume % or greater and 55 volume % or less, in which in a case where a total amount of the resin composition contained in the fiber-reinforced resin molding material is 100 mass %, a thickness from a first surface in a thickness direction of the fiber-reinforced resin molding material to a position occupied by 10 mass % of the resin composition is represented by d1 (μm), and a thickness from a second surface opposite to the first surface to a position occupied by 10 mass % of the resin composition is represented by d2 (μm), an absolute value (|d1−d2|) of a difference between d1 and d2 is 50 μm or less. A method for manufacturing a fiber-reinforced resin molding material, including: impregnating a reinforcement fiber sheet formed of at least one selected from the group consisting of a unidirectional sheet in which a plurality of continuous fibers are arranged in parallel in one direction, a woven fabric in which continuous fibers are woven, and a non-crimp fabric containing continuous fibers with a resin composition having an initial viscosity of 1 Pa·s or less and having a viscosity of 5,000 Pa·s or greater and 150,000 Pa·s or less after leaving for 7 days at 25° C.

## Claims

### Claim 1

A method for manufacturing a fiber-reinforced resin molding material, the method comprising:
coating of a resin composition on one surface of each of a first carrier film and a second carrier film, and
impregnation of a reinforced fiber sheet with the resin composition after the coating by overlaying the first and second carrier films so that the surfaces coated by the resin composition face each other and in a state that the reinforced fiber sheet is put between the first and second carrier films, and conveying while pressing with a plurality of pressing rolls,
wherein the reinforced fiber sheet is one selected from the group consisting of a unidirectional sheet in which a plurality of continuous fibers are arranged in parallel in one direction, a woven fabric in which continuous fibers are woven, and a non-crimp fabric comprising continuous fibers.

### Claim 2 (depends on 1)

The method of claim 1, wherein the resin composition has an initial viscosity of 1 Pa·s or less and a viscosity of 5,000 Pa·s or greater and 150,000 Pa·s or less after leaving for 7 days at 25° C.

### Claim 3 (depends on 1)

The method of claim 1, wherein the resin composition comprises at least one thermosetting resin selected from the group consisting of an epoxy resin, a vinyl ester resin, an unsaturated polyester resin, a polyimide resin, a maleimide resin, and a phenol resin.

### Claim 4 (depends on 3)

The method of claim 3, wherein the resin composition comprises a vinyl ester resin.

### Claim 5 (depends on 1)

The method of claim 1, wherein the continuous fibers are continuous fibers selected from the group consisting of carbon fibers, glass fibers, and aramid fibers.

### Claim 6 (depends on 1)

The method of claim 1, wherein the reinforced fiber sheet is a non-crimp fabric comprising continuous fibers.

### Claim 7 (depends on 1)

The method of claim 1, wherein the basis weight of the reinforcement fiber sheet is 200 g/m2 or greater and 3,000 g/m2 or less.

### Claim 8 (depends on 1)

The method of claim 1, wherein the reinforced fiber sheet is impregnated so that an amount of the resin composition in the fiber-reinforced resin molding material is 25 volume % or greater and 55 volume % or less.

### Claim 9 (depends on 1)

The method of claim 1, wherein the reinforced fiber sheet is a non-crimp fabric comprising continuous fibers,
wherein the basis weight of the reinforcement fiber sheet is 200 g/m2 or greater and 3,000 g/m2 or less, and
wherein the reinforced fiber sheet is impregnated so that an amount of the resin composition in the fiber-reinforced resin molding material is 25 volume % or greater and 55 volume % or less.

### Claim 10 (depends on 1)

The method of claim 1, wherein the basis weight of the reinforcement fiber sheet is 200 g/m2 or greater and 3,000 g/m2 or less,
wherein the reinforced fiber sheet is impregnated so that an amount of the resin composition in the fiber-reinforced resin molding material is 25 volume % or greater and 55 volume % or less, and
wherein, when a total amount of the resin composition contained in the fiber-reinforced resin molding material is 100 mass %, a thickness from a first surface in a thickness direction of the fiber-reinforced resin molding material to a position occupied by 10 mass % of the resin composition is represented by d1 (μm), and a thickness from a second surface opposite to the first surface to a position occupied by 10 mass % of the resin composition is represented by d2 (μm), an absolute value (|d1−d2|) of a difference between d1 and d2 is 50 μm or less.

### Claim 11 (depends on 10)

The method of claim 10, wherein R representing a ratio of the sum of d1 and d2 to the basis weight of the reinforcement fiber sheet is 0.2 or greater and 0.5 or less.

### Claim 12 (depends on 10)

The method of claim 10, wherein at least either of d1 and d2 is 5 μm or greater and 750 μm or less.

### Claim 13 (depends on 1)

The method of claim 1, wherein the resin composition has an initial viscosity of 1 Pa·s or less and a viscosity of 5,000 Pa·s or greater and 150,000 Pa·s or less after leaving for 7 days at 25° C., and
wherein the resin composition comprises at least one thermosetting resin selected from the group consisting of an epoxy resin, a vinyl ester resin, an unsaturated polyester resin, a polyimide resin, a maleimide resin, and a phenol resin.

### Claim 14 (depends on 1)

The method of claim 1, wherein the resin composition has an initial viscosity of 1 Pa·s or less and a viscosity of 5,000 Pa·s or greater and 150,000 Pa·s or less after leaving for 7 days at 25° C., and
wherein the resin composition comprises a vinyl ester resin.

### Claim 15 (depends on 1)

The method of claim 1, wherein the resin composition has an initial viscosity of 1 Pa·s or less and a viscosity of 5,000 Pa·s or greater and 150,000 Pa·s or less after leaving for 7 days at 25° C., and
wherein the reinforced fiber sheet is a non-crimp fabric comprising continuous fibers.

### Claim 16 (depends on 1)

The method of claim 1, wherein the resin composition has an initial viscosity of 1 Pa·s or less and a viscosity of 5,000 Pa·s or greater and 150,000 Pa·s or less after leaving for 7 days at 25° C.,
wherein the reinforced fiber sheet is a non-crimp fabric comprising continuous fibers, and
wherein the resin composition comprises a vinyl ester resin.

### Claim 17 (depends on 1)

The method of claim 1, wherein the resin composition has an initial viscosity of 1 Pa·s or less and a viscosity of 5,000 Pa·s or greater and 150,000 Pa·s or less after leaving for 7 days at 25° C.,
wherein the resin composition comprises a vinyl ester resin,
wherein the basis weight of the reinforcement fiber sheet is 200 g/m2 or greater and 3,000 g/m2 or less, and
wherein the reinforced fiber sheet is impregnated so that an amount of the resin composition in the fiber-reinforced resin molding material is 25 volume % or greater and 55 volume % or less.

### Claim 18 (depends on 1)

The method of claim 1, wherein the resin composition has an initial viscosity of 1 Pa·s or less and a viscosity of 5,000 Pa·s or greater and 150,000 Pa·s or less after leaving for 7 days at 25° C.,
wherein the reinforced fiber sheet is a non-crimp fabric comprising continuous fibers,
wherein the basis weight of the reinforcement fiber sheet is 200 g/m2 or greater and 3,000 g/m2 or less, and
wherein the reinforced fiber sheet is impregnated so that an amount of the resin composition in the fiber-reinforced resin molding material is 25 volume % or greater and 55 volume % or less.

### Claim 19 (depends on 1)

The method of claim 1, wherein the resin composition has an initial viscosity of 1 Pa·s or less and a viscosity of 5000 Pa·s or greater and 150,000 Pa·s or less after leaving for 7 days at 25° C.,
wherein the resin composition comprises a vinyl ester resin,
wherein the reinforced fiber sheet is a non-crimp fabric comprising continuous fibers,
wherein the basis weight of the reinforcement fiber sheet is 200 g/m2 or greater and 3,000 g/m2 or less, and
wherein the reinforced fiber sheet is impregnated so that an amount of the resin composition in the fiber-reinforced resin molding material is 25 volume % or greater and 55 volume % or less.

### Claim 20 (depends on 1)

The method of claim 1, wherein the resin composition has an initial viscosity of 1 Pa·s or less and a viscosity of 5,000 Pa·s or greater and 150,000 Pa·s or less after leaving for 7 days at 25° C.,
wherein the basis weight of the reinforcement fiber sheet is 200 g/m2 or greater and 3,000 g/m2 or less, and
wherein the reinforced fiber sheet is impregnated so that an amount of the resin composition in the fiber-reinforced resin molding material is 25 volume % or greater and 55 volume % or less.