# US 2021/0331265 A1 · Method for weld performance validation

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0331265 A1
- Document ID: US20210331265A1
- Status: Published application
- Kind: A1
- Application number: 16/857,373
- Filed: 2020-04-24
- Published: 2021-10-28
- Earliest claimed: 2020-04-24
- Assignees: GM Global Technology Operations LLC
- Applicants: GM Global Technology Operations LLC
- Inventors: Tingting Zhang; Spyros P. Mellas; Kangping Wang
- Web page: https://patentgrep.com/patent/US20210331265A1

## CPC

- B23K 9/095: Monitoring or automatic control of welding parameters
- B23K 31/02: relating to soldering or welding
- B23K 31/125: {Weld quality monitoring}
- G01N 3/02: Details
- G01N 3/08: by applying steady tensile or compressive forces (G01N3/28 takes precedence)
- G01N 2203/0017: Tensile
- G01N 2203/0282: Two dimensional, e.g. tapes, webs, sheets, strips, disks or membranes
- G01N 2203/0296: Welds
- B23K: SOLDERING OR UNSOLDERING; WELDING; CLADDING OR PLATING BY SOLDERING OR WELDING; CUTTING BY APPLYING HEAT LOCALLY, e.g. FLAME CUTTING; WORKING BY LASER BEAM
- G01N: INVESTIGATING OR ANALYSING MATERIALS BY DETERMINING THEIR CHEMICAL OR PHYSICAL PROPERTIES (measuring or testing apparatus or processes other than immunoassay, involving enzymes or microorganisms C12M, C12Q)

## Abstract

Methods are provided for joint performance validation and include preparing a coupon from a blank by bending the blank to have a pair of legs disposed at substantially ninety degrees relative to each other. Another coupon is prepared by forming an opening in a segment of another blank and bending the segment approximately ninety degrees. The segment is disposed adjacent an end of the second blank. A test sample is prepared by joining the coupons together at a joint with a leg attached to the segment approximately at a center of the leg. The test sample is subjected to a force test to generate data for the performance validation.

## Claims

### Claim 1

A method for joint performance validation, the method comprising:
fabricating a first coupon from a first blank including bending the first blank to have a first leg and a second leg disposed at substantially ninety degrees relative to the first leg;
fabricating a second coupon from a second blank including forming an opening in a segment of the second blank, wherein the segment is disposed adjacent an end of the second blank, and bending the segment approximately ninety degrees;
forming a test sample including joining the first coupon and the second coupon together at a joint with the first leg attached to the segment approximately at a center of the first leg; and
subjecting the test sample to a force test.

### Claim 2 (depends on 1)

The method of claim 1, wherein forming the opening comprises removing a corner at the end of the second blank so that the segment comprises a tab on the second coupon, and forming a radius adjacent the segment.

### Claim 3 (depends on 2)

The method of claim 2, comprising forming the radius to be greater than ten millimeters in size.

### Claim 4 (depends on 1)

The method of claim 1, wherein forming the opening comprises forming a slot in the segment.

### Claim 5 (depends on 1)

The method of claim 1, comprising:
recording force and displacement; and
characterizing, using the recorded force and displacement, the test sample.

### Claim 6 (depends on 1)

The method of claim 1, comprising forming the joint as a weld bead along an edge of the segment.

### Claim 7 (depends on 1)

The method of claim 1, wherein the first leg has a first width and the segment has a second width that is approximately half of the first width.

### Claim 8 (depends on 1)

The method of claim 1, comprising pulling the coupons apart by a test machine until separation of the coupons occurs.

### Claim 9 (depends on 8)

The method of claim 8, comprising:
characterizing the separation as one of a weld failure, a coupon parent material failure, and a heat affected zone failure; and
adjusting, when the coupon parent material failures occur, geometry of the coupons to align a location of the coupon parent material failure to a centerline of the coupons.

### Claim 10 (depends on 8)

The method of claim 8, comprising:
recording force and deflection; and
modeling the joint using the force and deflection.

### Claim 11

A method for joint performance validation, the method comprising:
fabricating a first coupon from a first blank by bending the first blank to have a first leg and a second leg disposed at substantially ninety degrees relative to the first leg;
fabricating a second coupon from a second blank by removing a portion of a segment of the second blank, wherein the segment is disposed adjacent an end of the second blank, and bending the segment approximately ninety degrees;
forming a test sample by joining the first coupon and the second coupon together at a joint that comprises a weld located approximately at a center of the first leg, with the first leg attached to the segment by the weld;
subjecting the test sample to a force test;
recording test data from the force test; and
evaluating the weld using the test data.

### Claim 12 (depends on 11)

The method of claim 11, wherein forming the opening comprises removing a corner at the end of the second blank so that the segment comprises a tab on the second coupon, and forming a radius extending from the tab.

### Claim 13 (depends on 11)

The method of claim 11, wherein forming the opening comprises forming a slot in the segment, wherein the slot is closed.

### Claim 14 (depends on 11)

The method of claim 11, comprising:
recording force and displacement; and
characterizing, using the recorded force and displacement, the weld.

### Claim 15 (depends on 11)

The method of claim 11, wherein the weld is formed as an elongated bead along an edge of the segment.

### Claim 16 (depends on 11)

The method of claim 11, wherein the first leg has a width and the segment extends to a point located at approximately half of the width.

### Claim 17 (depends on 11)

The method of claim 11, comprising pulling the coupons apart by a test machine until separation of the coupons occurs.

### Claim 18 (depends on 17)

The method of claim 17, comprising characterizing the separation as one of a weld failure, a coupon failure, and a heat affected zone failure.

### Claim 19 (depends on 18)

The method of claim 18, comprising:
recording force and deflection; and
modeling the joint using the force and deflection.

### Claim 20

A method for joint performance validation, the method comprising:
determining material composition and weld parameters for a product;
fabricating a first coupon and a second coupon using the material composition;
fabricating the first coupon from a first blank by bending the first blank to have a first leg and a second leg disposed at substantially ninety degrees relative to the first leg;
fabricating the second coupon from a second blank by removing a portion of a segment of the second blank, wherein the segment is disposed adjacent an end of the second blank, and bending the segment approximately ninety degrees;
forming a test sample by joining the first coupon and the second coupon together at a joint that comprises a weld located approximately at a center of the first leg, with the first leg attached to the segment by the weld, wherein the weld is formed using the weld parameters;
performing a force test on the test sample;
recording force and deflection of the test sample; and
modeling the joint using the recorded force and deflection.