# US 2021/0331239 A1 · Method for Manufacturing Nickel-Based Alloy Repaired Member

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0331239 A1
- Document ID: US20210331239A1
- Status: Published application
- Kind: A1
- Application number: 17/158,822
- Filed: 2021-01-26
- Published: 2021-10-28
- Earliest claimed: 2020-04-24
- Assignees: Mitsubishi Power, Ltd.
- Applicants: Mitsubishi Power, Ltd.
- Inventors: Takeshi IZUMI; Atsuo OTA
- Web page: https://patentgrep.com/patent/US20210331239A1

## CPC

- B22F 7/062: {involving the connection or repairing of preformed parts}
- B22F 3/115: by spraying molten metal, i.e. spray sintering, spray casting
- B22F 3/24: After-treatment of workpieces or articles {(B22F3/1146 takes precedence)}
- B23P 6/007: {using only additive methods, e.g. build-up welding}
- C22C 19/055: {with the maximum Cr content being at least 20% but less than 30%}
- C22C 19/056: {with the maximum Cr content being at least 10% but less than 20%}
- C22C 19/057: {with the maximum Cr content being less 10%}
- C22F 1/10: of nickel or cobalt or alloys based thereon
- C23C 4/02: Pretreatment of the material to be coated, e.g. for coating on selected surface areas
- C23C 4/06: Metallic material
- C23C 4/073: containing MCrAl or MCrAlY alloys, where M is nickel, cobalt or iron, with or without non-metal elements
- C23C 4/08: containing only metal elements (C23C4/073 takes precedence)
- C23C 4/129: Flame spraying
- C23C 4/18: After-treatment
- C23C 24/08: by application of heat or pressure and heat (C23C24/04 takes precedence)
- C23C 24/082: {without intermediate formation of a liquid in the layer}
- C23C 24/087: {Coating with metal alloys or metal elements only}
- F01D 5/005: {Repairing methods or devices}
- B22F 2003/248: {Thermal after-treatment}
- B22F 2007/068: {repairing articles}
- B22F 2203/11: temperature, temperature profile
- B22F 2301/15: Nickel or cobalt
- B22F 2301/155: Rare Earth - Co or -Ni intermetallic alloys
- F05D 2230/31: Layer deposition
- F05D 2230/311: by torch or flame spraying
- F05D 2230/40: Heat treatment
- F05D 2300/17: Alloys
- Y02T 50/60: Efficient propulsion technologies, e.g. for aircraft
- B22F: WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER (making alloys by powder metallurgy C22C); APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B23P: METAL-WORKING NOT OTHERWISE PROVIDED FOR; COMBINED OPERATIONS; UNIVERSAL MACHINE TOOLS (arrangements for copying or controlling B23Q)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- F01D: NON-POSITIVE DISPLACEMENT MACHINES OR ENGINES, e.g. STEAM TURBINES (machines or engines for liquids F03; non-positive displacement pumps F04D)
- F05D: INDEXING SCHEME FOR ASPECTS RELATING TO NON-POSITIVE-DISPLACEMENT MACHINES OR ENGINES, GAS-TURBINES OR JET-PROPULSION PLANTS
- Y02T: CLIMATE CHANGE MITIGATION TECHNOLOGIES RELATED TO TRANSPORTATION

## Abstract

There is provided a manufacturing method of a Ni-based alloy repaired member having a repair piece formed at a damaged portion of a base material. The base material and the repair piece are made of a high precipitation-strengthened Ni-based alloy material. The manufacturing method includes the steps of: preprocessing a surface of the damaged portion; preparing a Ni-based alloy powder having a predetermined chemical composition; depositing a sprayed piece on the damaged portion by a high-speed collision spraying process using the Ni-based alloy powder; subjecting the sprayed piece to a predetermined heat treatment so that the sprayed piece is thermally refined to a softened sprayed piece; processing the softened sprayed piece into a shaped sprayed piece with a desired shape; and subjecting whole of the shaped sprayed piece and the base material to a predetermined heat treatment so that the shaped sprayed piece is thermally refined to the repair piece.

## Claims

### Claim 1

A manufacturing method of a Ni-based alloy repaired member in that a repair piece is formed at a damaged portion of a base material, each of the base material and the repair piece being made of a Ni-based alloy having a chemical composition in which the equilibrium amount of precipitation of a ′ phase precipitating in a phase of matrix at 700° C. is 30 volume % or more and 80 volume % or less,
the manufacturing method comprising:
a damaged portion surface preparation step for preprocessing a surface of the damaged portion;
an alloy powder preparation step for preparing a Ni-based alloy powder having the chemical composition;
a sprayed piece deposition step for depositing/forming a sprayed piece on the damaged portion by a high-speed collision spraying process using the Ni-based alloy powder;
a softening heat treatment step for heating the sprayed piece to a temperature equal to or higher than the solvus temperature of the ′ phase but lower than the melting temperature of the phase, and then slow-cooling the heated sprayed piece from the temperature to a temperature at least 50° C. lower than the ′ phase solvus temperature at a cooling rate of 100° C./h or lower, so that the sprayed piece is thermally refined to a softened sprayed piece in that particles of the ′ phase at least 20 volume % precipitate on grain boundaries of the phase grains having an average grain diameter of 50 μm or less;
a shaping step for processing the softened sprayed piece into a shaped sprayed piece with a desired shape by cold plastic working, warm plastic working and/or machining; and
a solution and aging heat treatment step for subjecting whole of the shaped sprayed piece and the base material to a solution heat treatment so as to solid-dissolve the ′ phase into the phase and subsequently subjecting it to an aging heat treatment so as to precipitate particles of the ′ phase of at least 30 volume % within the phase grains, so that the shaped sprayed piece is thermally refined to the repair piece.

### Claim 2 (depends on 1)

The manufacturing method according to claim 1, wherein
the high-speed collision spraying process is a high velocity oxy-fuel spraying, a high velocity air-fuel spraying or a cold spraying.

### Claim 3 (depends on 1)

The manufacturing method according to claim 1, wherein
the softened sprayed piece has a Vickers hardness of 390 Hv or less at a room temperature.

### Claim 4 (depends on 1)

The manufacturing method according to claim 1, wherein
the alloy powder preparation step includes an atomization substep for forming the Ni-based alloy powder.

### Claim 5 (depends on 1)

The manufacturing method according to claim 1, wherein
the chemical composition of the repair piece is:
5 mass % to 25 mass % of Cr,
more than 0 mass % to 30 mass % of Co,
1 mass % to 8 mass % of Al,
1 mass % to 10 mass % of Ti, Nb and Ta in total,
10 mass % or less of Fe,
10 mass % or less of Mo,
8 mass % or less of W,
0.1 mass % or less of Zr,
0.1 mass % or less of B,
0.2 mass % or less of C,
2 mass % or less of Hf,
5 mass % or less of Re,
0.003 mass % to 0.05 mass % of O, and
residual components of Ni and unavoidable impurities.

### Claim 6 (depends on 1)

The manufacturing method according to claim 1, wherein
each of the base material and the repair piece has a chemical composition in which the solvus temperature of the ′ phase is 1110° C. or higher.

### Claim 7 (depends on 6)

The manufacturing method according to claim 6, wherein
each of the base material and the repair piece has a chemical composition in which the equilibrium amount of precipitation of the ′ phase at 700° C. is 45 volume % or more and 80 volume % or less.

### Claim 8 (depends on 1)

The manufacturing method according to claim 1, wherein
the based material is a unidirectional solidification article or a single crystalline solidification article comprising the phase, and
the solution heat treatment is a solution/non-recrystallization heat treatment in which the whole of the shaped sprayed piece and the base material is held at a temperature at least 10° C. higher than the solvus temperature of the ′ phase but not higher than a temperature that is 10° C. lower than the melting point of the phase, for a holding duration within a time range in which recrystallized grains of the phase do not generate.

### Claim 9 (depends on 8)

The manufacturing method according to claim 8, wherein
the holding duration in the solution/non-recrystallization heat treatment step is within a range from 15 minutes to 2 hours.