# US 2021/0288381 A1 · Polymer composite membrane, preparation method for same, and lithium-ion battery including same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0288381 A1
- Document ID: US20210288381A1
- Status: Published application
- Kind: A1
- Application number: 16/328,601
- Filed: 2017-08-14
- Published: 2021-09-16
- Earliest claimed: 2016-08-29
- Assignees: BYD Company Limited
- Applicants: BYD Company Limited
- Inventors: Jialing HU; Jun SHAN; Jinxiang WU; Long HE
- Web page: https://patentgrep.com/patent/US20210288381A1

## CPC

- H01M 10/052: Li-accumulators
- H01M 50/454: comprising a non-fibrous layer and a fibrous layer superimposed on one another
- H01M 50/403: Manufacturing processes of separators, membranes or diaphragms
- H01M 50/414: Synthetic resins, e.g. thermoplastics or thermosetting resins
- H01M 50/417: Polyolefins
- H01M 50/42: Acrylic resins
- H01M 50/423: Polyamide resins
- H01M 50/426: Fluorocarbon polymers
- H01M 50/434: Ceramics
- H01M 50/44: Fibrous material
- H01M 50/451: comprising layers of only organic material and layers containing inorganic material
- H01M 50/457: comprising three or more layers
- H01M 50/461: {with adhesive layers between electrodes and separators}
- H01M 50/491: Porosity
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY

## Abstract

The disclosure relates to the field of lithium-ion batteries, and discloses a polymer composite membrane and a method for preparing same. The disclosure further includes a lithium-ion battery for which the foregoing polymer composite membrane is used. The polymer composite membrane includes a porous base membrane and a heat-resistant fiber layer covering at least one side surface of the porous base membrane, where materials of the heat-resistant fiber layer contain a first polymeric material and a second polymeric material.

## Claims

### Claim 1

A polymer composite membrane,
comprising a porous base membrane; and
a heat-resistant fiber layer covering at least one side surface of the porous base membrane, wherein materials of the heat-resistant fiber layer contain a first polymeric material and a second polymeric material; the first polymeric material is a heat-resistant polymeric material whose melting point is above 180° C.; and the melting point of the second polymeric material is lower than that of the first polymeric material, and a liquid absorption rate of the second polymeric material in an electrolyte at 25° C. is above 40% and has an error of ±5%.

### Claim 2 (depends on 1)

The polymer composite membrane according to claim 1, wherein a liquid absorption rate of the first polymeric material in an electrolyte at 25° C. is below 5% and has an error of ±5%; and a liquid absorption rate of the second polymeric material in an electrolyte at 25° C. is 40% to 100% and has an error of ±5%.

### Claim 3 (depends on 1)

The polymer composite membrane according to claim 1, wherein the glass transition temperature of the first polymeric material is above 100° C.; and the melting point of the second polymeric material is 100° C. to 150° C.; and optionally, the glass transition temperature of the second polymeric material is below 25° C.

### Claim 4

(canceled)

### Claim 5

(canceled)

### Claim 6 (depends on 1)

The polymer composite membrane according to claim 1, wherein the materials of the heat-resistant fiber layer are a mixture of the first polymeric material and the second polymeric material.

### Claim 7 (depends on 1)

The polymer composite membrane according to claim 1, wherein a weight ratio between the first polymeric material and the second polymeric material in the heat-resistant fiber layer is (0.5 to 10):1.

### Claim 8 (depends on 1)

The polymer composite membrane according to claim 1, wherein
the first polymeric material is selected from one or more of polyetherimide, poly(ether ether ketone), polyether sulfone, polyamide-imide, polyamide acid, and polyvinylpyrrolidone; and
the second polymeric material is selected from one or more of modified polyvinylidene fluoride, polyacrylate, polyphenyl ethylene, and polyethylene oxide; optionally, the modified polyvinylidene fluoride is polyvinylidene fluoride-hexafluoropropylene; and optionally, the polyacrylate is selected from one or more of polymethyl acrylate, polyethylene acrylate, and polymethyl methacrylate.

### Claim 9 (depends on 8)

The polymer composite membrane according to claim 8, wherein the first polymeric material is polyetherimide, and the second polymeric material is polyvinylidene fluoride-hexafluoropropylene; and optionally, the materials of the heat-resistant fiber layer are a mixture of polyetherimide and polyvinylidene fluoride-hexafluoropropylene.

### Claim 10 (depends on 1)

The polymer composite membrane according to claim 1, wherein the diameter of fiber in the heat-resistant fiber layer is 100 nm to 2000 nm, and the thickness of the heat-resistant fiber layer is 0.5 μm to 30 μm.

### Claim 11 (depends on 1)

The polymer composite membrane according to claim 1, wherein the heat-resistant fiber layer has a porosity of 75% to 93% and a surface density of 0.2 g/m2 to 15 g/m2.

### Claim 12 (depends on 1)

The polymer composite membrane according to claim 1, wherein the porous base membrane is a polymer base membrane or a ceramic membrane, and the ceramic membrane comprises a polymer base membrane and a ceramic layer that is formed on at least a side surface of the polymer base membrane;
the porous base membrane is a ceramic membrane, and the heat-resistant fiber layer is located on a surface on a side of the ceramic membrane on which a ceramic layer is formed; and
the polymer base membrane is a polyolefin membrane.

### Claim 13 (depends on 10)

The polymer composite membrane according to claim 10, wherein the ceramic layer contains ceramic particles and a binder, and a surface density p of the ceramic layer at a thickness of 1 μm satisfies 1.8 mg/cm2<ρ≤2.7 mg/cm2;
the ceramic particle is selected from one or more of Al2O3, SiO2, BaSO4, BaO, TiO2, CuO, MgO, Mg(OH)2, LiAlO2, ZrO2, CNT, BN, SiC, Si3N4, WC, BC, AlN, Fe2O3, BaTiO3, MoS2, α-V2O5, PbTiO3, TiB2, CaSiO3, molecular sieve, clay, boehmite, and kaolin, and optionally, an average particle size of the ceramic particle is 200 nm to 800 nm;
the binder is polyacrylate whose glass transition temperature satisfies −40° C. to 0° C.; and
the single-sided thickness of the ceramic layer is 1 μm to 5 μm.

### Claim 14 (depends on 11)

The polymer composite membrane according to claim 11, wherein in the ceramic layer, relative to the ceramic particles of 100 parts by weight, the content of the binder is 2 to 8 parts by weight;
in the ceramic layer, relative to the ceramic particles of 100 parts by weight, a dispersant of 0.3 to 1 part by weight, a thickener of 0.5 to 1.8 parts by weight, and a surface treating agent of 0 to 1.5 parts by weight are further comprised, and the number-average molecular weight of the dispersant is below 50000;
in the ceramic layer, relative to the ceramic particles of 100 parts by weight, the content of the binder is 4 to 6 parts by weight, the content of the dispersant is 0.4 to 0.8 part by weight, the content of the thickener is 0.7 to 1.5 parts by weight, and the content of the surface treating agent is 0.5 to 1.2 parts by weight;
the dispersant is at least one of polyacrylate, aliphatic polyglycol ether, silicates, phosphates, and guar gum;
the thickener is at least one of polyacrylate, a polyacrylate copolymer, polyvinylpyrrolidone, a cellulose derivative, and polyacrylamide; and
the surface treating agent is 3-glycidyloxypropyltrimethoxysilane and/or 3-glycidyloxypropyltriethoxysilane.

### Claim 15 (depends on 1)

The polymer composite membrane according to claim 1, wherein the polymer composite membrane further comprises a bonding layer, the bonding layer is formed on an outermost side of at least one side surface of the polymer composite membrane, the bonding layer contains an acrylate crosslinked polymer, a styrene-acrylate crosslinked copolymer and a vinylidene fluoride-hexafluoropropylene copolymer, or the bonding layer contains an acrylate crosslinked polymer and a styrene-acrylate crosslinked copolymer, or the bonding layer contains an acrylate crosslinked polymer and a vinylidene fluoride-hexafluoropropylene copolymer, and the porosity of the bonding layer is 40% to 65%; and
the glass transition temperature of the acrylate crosslinked polymer is −20° C. to 60° C., the glass transition temperature of the styrene-acrylate crosslinked copolymer is −30° C. to 50° C., and the glass transition temperature of the vinylidene fluoride-hexafluoropropylene copolymer is −65° C. to −40° C.

### Claim 16 (depends on 15)

The polymer composite membrane according to claim 15, wherein
the bonding layer contains the acrylate crosslinked polymer and the styrene-acrylate crosslinked copolymer and does not contain the vinylidene fluoride-hexafluoropropylene copolymer, and a weight ratio of the acrylate crosslinked polymer to the styrene-acrylate crosslinked copolymer is 1:(0.05 to 2); or
the bonding layer contains the acrylate crosslinked polymer and the vinylidene fluoride-hexafluoropropylene copolymer and does not contain the styrene-acrylate crosslinked copolymer, and a weight ratio of the acrylate crosslinked polymer to the vinylidene fluoride-hexafluoropropylene copolymer is 1:(0.3 to 25); or
the bonding layer contains the acrylate crosslinked polymer, the styrene-acrylate crosslinked copolymer, and the vinylidene fluoride-hexafluoropropylene copolymer, and a weight ratio between the acrylate crosslinked polymer, the styrene-acrylate crosslinked copolymer and the vinylidene fluoride-hexafluoropropylene copolymer is 1:(0.01 to 2):(0.3 to 5).

### Claim 17 (depends on 15)

The polymer composite membrane according to claim 15, wherein the acrylate crosslinked polymer is a mixture of a first acrylate crosslinked polymer and a second acrylate crosslinked polymer and/or a third acrylate crosslinked polymer, or a second acrylate crosslinked polymer, or a third acrylate crosslinked polymer;
the first acrylate crosslinked polymer contains a polymethyl methacrylate chain segment of 70 to 80 wt %, a polyethylene acrylate chain segment of 2 to 10 wt %, a polybutyl acrylate chain segment of 10 to 20 wt %, and a polyacrylic acid chain segment of 2 to 10 wt %, the second acrylate crosslinked polymer contains a polymethyl methacrylate chain segment of 30 to 40 wt %, a polyethylene acrylate chain segment of 2 to 10 wt %, a polybutyl acrylate chain segment of 50 to 60 wt %, and a polyacrylic acid chain segment of 2 to 10 wt %, and the third acrylate crosslinked polymer contains a polymethyl methacrylate chain segment of 50 to 80 wt %, a polyethylene acrylate chain segment of 2 to 10 wt %, a polybutyl acrylate chain segment of 15 to 40 wt %, and a polyacrylic acid chain segment of 2 to 10 wt %; the glass transition temperature of the first acrylate crosslinked polymer is 50° C. to 60° C., the glass transition temperature of the second acrylate crosslinked polymer is −20° C. to −5° C., and the glass transition temperature of the third acrylate crosslinked polymer is 30° C. to 50° C.;
the styrene-acrylate crosslinked copolymer contains a polyphenyl ethylene chain segment of 40 to 50 wt %, a polymethyl methacrylate chain segment of 5 to 15 wt %, a polyethylene acrylate chain segment of 2 to 10 wt %, a polybutyl acrylate chain segment of 30 to 40 wt %, and a polyacrylic acid chain segment of 2 to 10 wt %; and the glass transition temperature of the styrene-acrylate crosslinked copolymer is 15° C. to 30° C.; and
the vinylidene fluoride-hexafluoropropylene copolymer contains a polyvinylidene fluoride chain segment of 80 to 98 wt % and a polyhexafluoropropylene chain segment of 2 to 20 wt %; and the glass transition temperature of the vinylidene fluoride-hexafluoropropylene copolymer is −60° C. to −40° C.

### Claim 18 (depends on 15)

The polymer composite membrane according to claim 15, wherein
the bonding layer contains a first acrylate crosslinked polymer, a second acrylate crosslinked polymer, and the styrene-acrylate crosslinked copolymer and does not contain the vinylidene fluoride-hexafluoropropylene copolymer, and a weight ratio between the first acrylate crosslinked polymer, the second acrylate crosslinked polymer and the styrene-acrylate crosslinked copolymer is (5 to 10):1:(10 to 13); or
the bonding layer contains the first acrylate crosslinked polymer, the second acrylate crosslinked polymer, and the vinylidene fluoride-hexafluoropropylene copolymer and does not contain the styrene-acrylate crosslinked copolymer, and a weight ratio between the first acrylate crosslinked polymer, he second acrylate crosslinked polymer and the vinylidene fluoride-hexafluoropropylene copolymer is (5 to 15):1:(5 to 12); or
the bonding layer contains the second acrylate crosslinked polymer and the vinylidene fluoride-hexafluoropropylene copolymer and does not contain the styrene-acrylate crosslinked copolymer, and a weight ratio between the second acrylate crosslinked polymer and the vinylidene fluoride-hexafluoropropylene copolymer is 1:(5 to 20); or
the bonding layer contains the second acrylate crosslinked polymer, the styrene-acrylate crosslinked copolymer, and the vinylidene fluoride-hexafluoropropylene copolymer, and a weight ratio between the second acrylate crosslinked polymer to, the styrene-acrylate crosslinked copolymer, and the vinylidene fluoride-hexafluoropropylene copolymer is 1:(0.5 to 2):(1 to 5); or
the bonding layer contains a third acrylate crosslinked polymer, the styrene-acrylate crosslinked copolymer, and the vinylidene fluoride-hexafluoropropylene copolymer, and a weight ratio between the third acrylate crosslinked polymer, the styrene-acrylate crosslinked copolymer, and the vinylidene fluoride-hexafluoropropylene copolymer is 1:(0.5 to 2):(1 to 5); or
the bonding layer contains the first acrylate crosslinked polymer, the second acrylate crosslinked polymer, the styrene-acrylate crosslinked copolymer, and the vinylidene fluoride-hexafluoropropylene copolymer, and a weight ratio between the first acrylate crosslinked polymer, the second acrylate crosslinked polymer, the styrene-acrylate crosslinked copolymer; and the vinylidene fluoride-hexafluoropropylene copolymer is (10 to 15):1:(0.5 to 2):(5 to 10), wherein
the first acrylate crosslinked polymer contains a polymethyl methacrylate chain segment of 70 to 80 wt %, a polyethylene acrylate chain segment of 2 to 10 wt %, a polybutyl acrylate chain segment of 10 to 20 wt %, and a polyacrylic acid chain segment of 2 to 10 wt %, the second acrylate crosslinked polymer contains a polymethyl methacrylate chain segment of 30 to 40 wt %, a polyethylene acrylate chain segment of 2 to 10 wt %, a polybutyl acrylate chain segment of 50 to 60 wt %, and a polyacrylic acid chain segment of 2 to 10 wt %, and the third acrylate crosslinked polymer contains a polymethyl methacrylate chain segment of 50 to 80 wt %, a polyethylene acrylate chain segment of 2 to 10 wt %, a polybutyl acrylate chain segment of 15 to 40 wt %, and a polyacrylic acid chain segment of 2 to 10 wt %; the styrene-acrylate crosslinked copolymer contains a polyphenyl ethylene chain segment of 40 to 50 wt %, a polymethyl methacrylate chain segment of 5 to 15 wt %, a polyethylene acrylate chain segment of 2 to 10 wt %, a polybutyl acrylate chain segment of 30 to 40 wt %, and a polyacrylic acid chain segment of 2 to 10 wt %; the vinylidene fluoride-hexafluoropropylene copolymer contains a polyvinylidene fluoride chain segment of 80 to 98 wt % and a polyhexafluoropropylene chain segment of 2 to 20 wt %; and the glass transition temperature of the first acrylate crosslinked polymer is 50° C. to 60° C., the glass transition temperature of the second acrylate crosslinked polymer is −20° C. to −5° C., the glass transition temperature of the third acrylate crosslinked polymer is 30° C. to 50° C., the glass transition temperature of the styrene-acrylate crosslinked copolymer is 15° C. to 30° C., and the glass transition temperature of the vinylidene fluoride-hexafluoropropylene copolymer is −60° C. to −40° C.

### Claim 19 (depends on 15)

The polymer composite membrane according to claim 15, wherein the bonding layer further contains at least one of an acrylonitrile-acrylate copolymer, a vinyl chloride-propylene copolymer, and a butadiene-styrene copolymer;
when the bonding layer further contains the acrylonitrile-acrylate copolymer, and a weight ratio between the acrylonitrile-acrylate copolymer and the acrylate crosslinked polymer is (0.05 to 2):1;
when the bonding layer further contains the vinyl chloride-propylene copolymer, and a weight ratio between the vinyl chloride-propylene copolymer and the acrylate crosslinked polymer is (0.15 to 7):1; and
when the bonding layer further contains the butadiene-styrene copolymer, and a weight ratio between the butadiene-styrene copolymer and the acrylate crosslinked polymer is (0.05 to 2):1.

### Claim 20 (depends on 15)

The polymer composite membrane according to claim 15, wherein the single-sided surface density of the bonding layer is 0.05 mg/cm2 to 0.9 mg/cm2; and the single-sided thickness of the bonding layer is 0.1 μm to 1 μm.

### Claim 21

A method for preparing a polymer composite membrane, comprising the following steps:
S1: providing a porous base membrane; and
S2: preparing a spinning solution containing a first polymeric material and a second polymeric material, and forming a heat-resistant fiber layer on at least one side surface of the porous base membrane through electrostatic spinning by using the spinning solution, wherein the first polymeric material is a heat-resistant polymeric material whose melting point is above 180° C.; and the melting point of the second polymeric material is lower than that of the first polymeric material, and a liquid absorption rate of the second polymeric material in an electrolyte at 25° C. is above 40% and has an error of ±5%;
a liquid absorption rate of the first polymeric material in an electrolyte at 25° C. is below 5% and has an error of ±5%;
the glass transition temperature of the first polymeric material is above 100° C.;
the melting point of the second polymeric material is 100° C. to 150° C.; and optionally, the glass transition temperature of the second polymeric material is below 25° C.; and
a liquid absorption rate of the second polymeric material in an electrolyte at 25° C. is 40% to 100% and has an error of ±5%.

### Claim at position 22

-38. (canceled)

### Claim 39 (depends on 1)

A lithium-ion battery, comprising a positive electrode, a negative electrode, and a battery membrane located between the positive electrode and the negative electrode, wherein the battery membrane is the polymer composite membrane according to claim 1.