# US 2021/0280946 A1 · Battery separator, lithium-ion battery, and preparation methods thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0280946 A1
- Document ID: US20210280946A1
- Status: Published application
- Kind: A1
- Application number: 16/319,602
- Filed: 2017-08-15
- Published: 2021-09-09
- Earliest claimed: 2016-08-29
- Assignees: BYD Company Limited
- Applicants: BYD Company Limited
- Inventors: Lina JIN; Jun SHAN; Gang HU; Long HE
- Web page: https://patentgrep.com/patent/US20210280946A1

## CPC

- H01M 50/451: comprising layers of only organic material and layers containing inorganic material
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- H01M 50/403: Manufacturing processes of separators, membranes or diaphragms
- H01M 50/417: Polyolefins
- H01M 50/42: Acrylic resins
- H01M 50/426: Fluorocarbon polymers
- H01M 50/449: having a layered structure
- H01M 50/457: comprising three or more layers
- H01M 50/491: Porosity
- Y02E 60/10: Energy storage using batteries
- Y02P 70/50: Manufacturing or production processes characterised by the final manufactured product
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

The present disclosure relates to the field of lithium-ion batteries, and discloses a battery separator and a lithium-ion battery, and preparation methods thereof. The battery separator includes a porous base membrane and a bonding layer attached to at least one side surface of the porous base membrane, wherein the bonding layer contains an acrylate crosslinked polymer and a styrene-acrylate crosslinked copolymer and/or a vinylidene fluoride-hexafluoropropylene copolymer, and the porosity of the bonding layer is 40-65%.

## Claims

### Claim 1

A battery separator, comprising
a porous base membrane, and
a bonding layer attached to at least one side surface of the porous base membrane,
wherein the bonding layer contains an acrylate crosslinked polymer and a styrene-acrylate crosslinked copolymer but does not contain a vinylidene fluoride-hexafluoropropylene copolymer, or the bonding layer contains an acrylate crosslinked polymer and a vinylidene fluoride-hexafluoropropylene copolymer but does not contain a styrene-acrylate crosslinked copolymer, or the bonding layer contains an acrylate crosslinked polymer, a styrene-acrylate crosslinked copolymer and a vinylidene fluoride-hexafluoropropylene copolymer, and
the porosity of the bonding layer is 40-65%.

### Claim 2 (depends on 1)

The battery separator according to claim 1, wherein the glass transition temperature of the acrylate crosslinked polymer is −20° C. to 60° C., the glass transition temperature of the styrene-acrylate crosslinked copolymer is −30° C. to 50° C., and the glass transition temperature of the vinylidene fluoride-hexafluoropropylene copolymer is −65° C. to −40° C.

### Claim 3 (depends on 1)

The battery separator according to claim 1, wherein
the weight ratio of the acrylate crosslinked polymer to the styrene-acrylate crosslinked copolymer is 1:0.05 to 1:2; or
the weight ratio of the acrylate crosslinked polymer to the vinylidene fluoride-hexafluoropropylene copolymer is 1:0.3 to 1:25; or
the weight ratio of the acrylate crosslinked polymer to the styrene-acrylate crosslinked copolymer to the vinylidene fluoride-hexafluoropropylene copolymer is 1:(0.01 to 2):(0.3 to 5).

### Claim 4 (depends on 1)

The battery separator according to claim 1, wherein the acrylate crosslinked polymer comprises a mixture of a first acrylate crosslinked polymer and a second acrylate crosslinked polymer and/or a third acrylate crosslinked polymer, or the second acrylate crosslinked polymer, or the third acrylate crosslinked polymer;
the first acrylate crosslinked polymer contains 70-80 wt % of polymethyl methacrylate segment, 2-10 wt % of polyethyl acrylate segment, 10-20 wt % of polybutyl acrylate segment and 2-10 wt % of polyacrylic acid segment, the second acrylate crosslinked polymer contains 30-40 wt % of polymethyl methacrylate segment, 2-10 wt % of polyethyl acrylate segment, 50-60 wt % of polybutyl acrylate segment and 2-10 wt % of polyacrylic acid segment, and the third acrylate crosslinked polymer contains 50-80 wt % of polymethyl methacrylate segment, 2-10 wt % of polyethyl acrylate segment, 15-40 wt % of polybutyl acrylate segment and 2-10 wt % of polyacrylic acid segment; and
the glass transition temperature of the first acrylate crosslinked polymer is 50° C. to 60° C., the glass transition temperature of the second acrylate crosslinked polymer is −20° C. to −5° C., and the glass transition temperature of the third acrylate crosslinked polymer is 30° C. to 50° C.

### Claim 5 (depends on 1)

The battery separator according to claim 1, wherein the styrene-acrylate crosslinked copolymer contains 40-50 wt % of polystyrene segment, 5-15 wt % of polymethyl methacrylate segment, 2-10 wt % of polyethyl acrylate segment, 30-40 wt % of polybutyl acrylate segment and 2-10 wt % of polyacrylic acid segment; and the glass transition temperature of the styrene-acrylate crosslinked copolymer is 15° C. to 30° C.

### Claim 6 (depends on 1)

The battery separator according to claim 1, wherein the vinylidene fluoride-hexafluoropropylene copolymer contains 80-98 wt % of polyvinylidene fluoride segment and 2-20 wt % of polyhexafluoropropylene segment; and the glass transition temperature of the vinylidene fluoride-hexafluoropropylene copolymer is −60° C. to −40° C.

### Claim 7 (depends on 4)

The battery separator according to claim 4, wherein
the bonding layer contains the first acrylate crosslinked polymer, the second acrylate crosslinked polymer and the styrene-acrylate crosslinked copolymer but does not contain the vinylidene fluoride-hexafluoropropylene copolymer, and the weight ratio of the first acrylate crosslinked polymer to the second acrylate crosslinked polymer to the styrene-acrylate crosslinked copolymer is (5 to 10):1:(10 to 13); or
the bonding layer contains the first acrylate crosslinked polymer, the second acrylate crosslinked polymer and the vinylidene fluoride-hexafluoropropylene copolymer but does not contain the styrene-acrylate crosslinked copolymer, and the weight ratio of the first acrylate crosslinked polymer to the second acrylate crosslinked polymer to the vinylidene fluoride-hexafluoropropylene copolymer is (5 to 15):1:(5 to 12); or
the bonding layer contains the second acrylate crosslinked polymer and the vinylidene fluoride-hexafluoropropylene copolymer but does not contain the styrene-acrylate crosslinked copolymer, and the weight ratio of the second acrylate crosslinked polymer to the vinylidene fluoride-hexafluoropropylene copolymer is 1:5 to 1:20; or
the bonding layer contains the second acrylate crosslinked polymer, the styrene-acrylate crosslinked copolymer and the vinylidene fluoride-hexafluoropropylene copolymer, and the weight ratio of the second acrylate crosslinked polymer to the styrene-acrylate crosslinked copolymer to the vinylidene fluoride-hexafluoropropylene copolymer is 1:(0.5 to 2):(1 to 5); or
the bonding layer contains the third acrylate crosslinked polymer, the styrene-acrylate crosslinked copolymer and the vinylidene fluoride-hexafluoropropylene copolymer, and the weight ratio of the third acrylate crosslinked polymer to the styrene-acrylate crosslinked copolymer to the vinylidene fluoride-hexafluoropropylene copolymer is 1:(0.5 to 2):(1 to 5); or, the bonding layer contains the first acrylate crosslinked polymer, the second acrylate crosslinked polymer, the styrene-acrylate crosslinked copolymer and the vinylidene fluoride-hexafluoropropylene copolymer, and the weight ratio of the first acrylate crosslinked polymer to the second acrylate crosslinked polymer to the styrene-acrylate crosslinked copolymer to the vinylidene fluoride-hexafluoropropylene copolymer is (10 to 15):1:(0.5 to 2):(5 to 10);
wherein the first acrylate crosslinked polymer contains 70-80 wt % of polymethyl methacrylate segment, 2-10 wt % of polyethyl acrylate segment, 10-20 wt % of polybutyl acrylate segment and 2-10 wt % of polyacrylic acid segment, the second acrylate crosslinked polymer contains 30-40 wt % of polymethyl methacrylate segment, 2-10 wt % of polyethyl acrylate segment, 50-60 wt % of polybutyl acrylate segment and 2-10 wt % of polyacrylic acid segment, the third acrylate crosslinked polymer contains 50-80 wt % of polymethyl methacrylate segment, 2-10 wt % of polyethyl acrylate segment, 15-40 wt % of polybutyl acrylate segment and 2-10 wt % of polyacrylic acid segment, the styrene-acrylate crosslinked copolymer contains 40-50 wt % of polystyrene segment, 5-15 wt % of polymethyl methacrylate segment, 2-10 wt % of polyethyl acrylate segment, 30-40 wt % of polybutyl acrylate segment and 2-10 wt % of polyacrylic acid segment, and the vinylidene fluoride-hexafluoropropylene copolymer contains 80-98 wt % of polyvinylidene fluoride segment and 2-20 wt % of polyhexafluoropropylene segment; and the glass transition temperature of the first acrylate crosslinked polymer is 50° C. to 60° C., the glass transition temperature of the second acrylate crosslinked polymer is −20° C. to −5° C., the glass transition temperature of the third acrylate crosslinked polymer is 30° C. to 50° C., the glass transition temperature of the styrene-acrylate crosslinked copolymer is 15° C. to 30° C., and the glass transition temperature of the vinylidene fluoride-hexafluoropropylene copolymer is −60° C. to −40° C.

### Claim 8 (depends on 1)

The battery separator according to claim 1, wherein the bonding layer further contains at least one of an acrylonitrile-acrylate copolymer, a chloroprene-acrylonitrile copolymer and a styrene-butadiene copolymer;
when the bonding layer further contains the acrylonitrile-acrylate copolymer, the weight ratio of the acrylonitrile-acrylate copolymer to the acrylate crosslinked polymer is 0.05:1 to 2:1;
when the bonding layer further contains the chloroprene-acrylonitrile copolymer, the weight ratio of the chloroprene-acrylonitrile copolymer to the acrylate crosslinked polymer is 0.15:1 to 7:1; and
when the bonding layer further contains the styrene-butadiene copolymer, the weight ratio of the styrene-butadiene copolymer to the acrylate crosslinked polymer is 0.05:1 to 2:1.

### Claim 9 (depends on 1)

The battery separator according to claim 1, wherein the single-side surface density of the bonding layer is 0.05-0.9 mg/cm2; and the single-side thickness of the bonding layer is 0.1-1 μm.

### Claim 10 (depends on 1)

The battery separator according to claim 1, wherein the porous base membrane is a polymer base membrane or a ceramic base membrane, and the ceramic base membrane comprises a polymer base membrane and a ceramic layer located on at least one side surface of the polymer base membrane; and the total thickness of the porous base membrane is 9-22 μm.

### Claim 11

A preparation method of a battery separator, comprising:
attaching a slurry containing a self-crosslinked pure acrylic emulsion and a self-crosslinked styrene-acrylic emulsion and/or a vinylidene fluoride-hexafluoropropylene copolymer emulsion to at least one side surface of a porous base membrane, and
drying to form a bonding layer having a porosity of 40-65% on at least one side surface of the porous base membrane.

### Claim 12 (depends on 11)

The method according to claim 11, wherein the glass transition temperature of the acrylate crosslinked polymer in the self-crosslinked pure acrylic emulsion is −20° C. to 60° C., the glass transition temperature of the styrene-acrylate crosslinked copolymer in the self-crosslinked styrene-acrylic emulsion is −30° C. to 50° C., and the glass transition temperature of the vinylidene fluoride-hexafluoropropylene copolymer in the vinylidene fluoride-hexafluoropropylene copolymer emulsion is −65° C. to −40° C.

### Claim 13 (depends on 11)

The method according to claim 11, wherein the slurry contains the self-crosslinked pure acrylic emulsion and the self-crosslinked styrene-acrylic emulsion but does not contain the vinylidene fluoride-hexafluoropropylene copolymer emulsion, and the weight ratio of solid content of the self-crosslinked pure acrylic emulsion to the self-crosslinked styrene-acrylic emulsion is 1:0.05 to 1:2; or
the slurry contains the self-crosslinked pure acrylic emulsion and the vinylidene fluoride-hexafluoropropylene copolymer emulsion but does not contain the self-crosslinked styrene-acrylic emulsion, and the weight ratio of solid content of the self-crosslinked pure acrylic emulsion to the vinylidene fluoride-hexafluoropropylene copolymer emulsion is 1:0.3 to 1:25; or
the slurry contains the self-crosslinked pure acrylic emulsion, the self-crosslinked styrene-acrylic emulsion and the vinylidene fluoride-hexafluoropropylene copolymer emulsion, and the weight ratio of solid content of the self-crosslinked pure acrylic emulsion to the self-crosslinked styrene-acrylic emulsion to the vinylidene fluoride-hexafluoropropylene copolymer emulsion is 1:(0.01 to 2):(0.3 to 5).

### Claim 14 (depends on 11)

The method according to claim 11, wherein the self-crosslinked pure acrylic emulsion is a mixture of a first self-crosslinked pure acrylic emulsion and a second self-crosslinked pure acrylic emulsion and/or a third self-crosslinked pure acrylic emulsion, or the second self-crosslinked pure acrylic emulsion, or the third self-crosslinked pure acrylic emulsion;
the acrylate crosslinked polymer in the first self-crosslinked pure acrylic emulsion contains 70-80 wt % of polymethyl methacrylate segment, 2-10 wt % of polyethyl acrylate segment, 10-20 wt % of polybutyl acrylate segment and 2-10 wt % of polyacrylic acid segment, the acrylate crosslinked polymer in the second self-crosslinked pure acrylic emulsion contains 30-40 wt % of polymethyl methacrylate segment, 2-10 wt % of polyethyl acrylate segment, 50-60 wt % of polybutyl acrylate segment and 2-10 wt % of polyacrylic acid segment, and the acrylate crosslinked polymer in the third self-crosslinked pure acrylic emulsion contains 50-80 wt % of polymethyl methacrylate segment, 2-10 wt % of polyethyl acrylate segment, 15-40 wt % of polybutyl acrylate segment and 2-10 wt % of polyacrylic acid segment; and
the glass transition temperature of the acrylate crosslinked polymer in the first self-crosslinked pure acrylic emulsion is 50° C. to 60° C., the glass transition temperature of the acrylate crosslinked polymer in the second self-crosslinked pure acrylic emulsion is −20° C. to −5° C., and the glass transition temperature of the acrylate crosslinked polymer in the third self-crosslinked pure acrylic emulsion is 30° C. to 50° C.

### Claim 15 (depends on 11)

The method according to claim 11, wherein the styrene-acrylate crosslinked copolymer in the self-crosslinked styrene-acrylic emulsion contains 40-50 wt % of polystyrene segment, 5-15 wt % of polymethyl methacrylate segment, 2-10 wt % of polyethyl acrylate segment, 30-40 wt % of polybutyl acrylate segment and 2-10 wt % of polyacrylic acid segment; and the glass transition temperature of the styrene-acrylate crosslinked copolymer is 15° C. to 30° C.

### Claim 16 (depends on 11)

The method according to claim 11, wherein the vinylidene fluoride-hexafluoropropylene copolymer in the vinylidene fluoride-hexafluoropropylene copolymer emulsion contains 80-98 wt % of polyvinylidene fluoride segment and 2-20 wt % of polyhexafluoropropylene segment; and the glass transition temperature of the vinylidene fluoride-hexafluoropropylene copolymer is −60° C. to −40° C.

### Claim 17 (depends on 11)

The method according to claim 11, wherein
the slurry contains the first self-crosslinked pure acrylic emulsion, the second self-crosslinked pure acrylic emulsion and the self-crosslinked styrene-acrylic emulsion but does not contain the vinylidene fluoride-hexafluoropropylene copolymer emulsion, and the weight ratio of solid content of the first self-crosslinked pure acrylic emulsion to the second self-crosslinked pure acrylic emulsion to the self-crosslinked styrene-acrylic emulsion is (5 to 10):1:(10 to 13); or
the slurry contains the first self-crosslinked pure acrylic emulsion, the second self-crosslinked pure acrylic emulsion and the vinylidene fluoride-hexafluoropropylene copolymer emulsion but does not contain the self-crosslinked styrene-acrylic emulsion, and the weight ratio of solid content of the first self-crosslinked pure acrylic emulsion to the second self-crosslinked pure acrylic emulsion to the vinylidene fluoride-hexafluoropropylene copolymer emulsion is (5 to 15):1:(5 to 12); or
the slurry contains the second self-crosslinked pure acrylic emulsion and the vinylidene fluoride-hexafluoropropylene copolymer emulsion but does not contain the self-crosslinked styrene-acrylic emulsion, and the weight ratio of solid content of the second self-crosslinked pure acrylic emulsion to the vinylidene fluoride-hexafluoropropylene copolymer emulsion is 1:5 to 1:20; or
the slurry contains the second self-crosslinked pure acrylic emulsion, the self-crosslinked styrene-acrylic emulsion and the vinylidene fluoride-hexafluoropropylene copolymer emulsion, and the weight ratio of solid content of the second self-crosslinked pure acrylic emulsion to the self-crosslinked styrene-acrylic emulsion to the vinylidene fluoride-hexafluoropropylene copolymer emulsion is 1:(0.5 to 2):(1 to 5); or
the slurry contains the third self-crosslinked pure acrylic emulsion, the self-crosslinked styrene-acrylic emulsion and the vinylidene fluoride-hexafluoropropylene copolymer emulsion, and the weight ratio of solid content of the third self-crosslinked pure acrylic emulsion to the self-crosslinked styrene-acrylic emulsion to the vinylidene fluoride-hexafluoropropylene copolymer emulsion is 1:(0.5 to 2):(1 to 5); or
the slurry contains the first self-crosslinked pure acrylic emulsion, the second self-crosslinked pure acrylic emulsion, the self-crosslinked styrene-acrylic emulsion and the vinylidene fluoride-hexafluoropropylene copolymer emulsion, and the weight ratio of solid content of the first self-crosslinked pure acrylic emulsion to the second self-crosslinked pure acrylic emulsion to the self-crosslinked styrene-acrylic emulsion to the vinylidene fluoride-hexafluoropropylene copolymer emulsion is (10 to 15):1:(0.5 to 2):(5 to 10);
the acrylate crosslinked polymer in the first self-crosslinked pure acrylic emulsion contains 70-80 wt % of polymethyl methacrylate segment, 2-10 wt % of polyethyl acrylate segment, 10-20 wt % of polybutyl acrylate segment and 2-10 wt % of polyacrylic acid segment, the acrylate crosslinked polymer in the second self-crosslinked pure acrylic emulsion contains 30-40 wt % of polymethyl methacrylate segment, 2-10 wt % of polyethyl acrylate segment, 50-60 wt % of polybutyl acrylate segment and 2-10 wt % of polyacrylic acid segment, the acrylate crosslinked polymer in the third self-crosslinked pure acrylic emulsion contains 50-80 wt % of polymethyl methacrylate segment, 2-10 wt % of polyethyl acrylate segment, 15-40 wt % of polybutyl acrylate segment and 2-10 wt % of polyacrylic acid segment, the styrene-acrylate crosslinked copolymer in the self-crosslinked styrene-acrylic emulsion contains 40-50 wt % of polystyrene segment, 5-15 wt % of polymethyl methacrylate segment, 2-10 wt % of polyethyl acrylate segment, 30-40 wt % of polybutyl acrylate segment and 2-10 wt % of polyacrylic acid segment, and the vinylidene fluoride-hexafluoropropylene copolymer in the vinylidene fluoride-hexafluoropropylene copolymer emulsion contains 80-98 wt % of polyvinylidene fluoride segment and 2-20 wt % of polyhexafluoropropylene segment; and the glass transition temperature of the acrylate crosslinked polymer in the first self-crosslinked pure acrylic emulsion is 50° C. to 60° C., the glass transition temperature of the acrylate crosslinked polymer in the second self-crosslinked pure acrylic emulsion is −20° C. to −5° C., the glass transition temperature of the acrylate crosslinked polymer in the third self-crosslinked pure acrylic emulsion is 30° C. to 50° C., the glass transition temperature of the styrene-acrylate crosslinked copolymer is 15° C. to 30° C., and the glass transition temperature of the vinylidene fluoride-hexafluoropropylene copolymer is −60° C. to −40° C.

### Claim 18 (depends on 11)

The method according to claim 11, wherein the slurry further contains at least one of an acrylonitrile-acrylate copolymer emulsion, an chloroprene-acrylonitrile emulsion and a styrene-butadiene latex;
when the slurry further contains the acrylonitrile-acrylate copolymer emulsion, the weight ratio of solid content of the acrylonitrile-acrylate copolymer emulsion to the self-crosslinked pure acrylic emulsion is 0.05:1 to 2:1;
when the slurry further contains the chloroprene-acrylonitrile emulsion, the weight ratio of solid content of the chloroprene-acrylonitrile emulsion to the self-crosslinked pure acrylic emulsion is 0.15:1 to 7:1; and
when the slurry further contains the styrene-butadiene latex, the weight ratio of solid content of the styrene-butadiene latex to the self-crosslinked pure acrylic emulsion is 0.05:1 to 2:1.

### Claim 19 (depends on 11)

The method according to claim 11, wherein an attaching method is a spraying method and/or a screen printing method; the operating temperatures of the spraying method and the screen printing method are each independently 30° C. to 80° C.; and the drying temperature is 30° C. to 80° C.

### Claim 20

(canceled)

### Claim 21 (depends on 1)

A lithium-ion battery, comprising a positive electrode plate, a negative electrode plate, an electrolyte and a battery separator according to claim 1.

### Claim 22

(canceled)