# US 2021/0280857 A1 · Composite graphite material, secondary battery, apparatus and preparation method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0280857 A1
- Document ID: US20210280857A1
- Status: Published application
- Kind: A1
- Application number: 17/330,400
- Filed: 2021-05-25
- Published: 2021-09-09
- Earliest claimed: 2019-12-03
- Assignees: Contemporary Amperex Technology Co., Limited
- Applicants: Contemporary Amperex Technology Co., Limited
- Inventors: Chengdu LIANG; Yuzhen ZHAO; Yan WEN; Qisen HUANG
- Web page: https://patentgrep.com/patent/US20210280857A1

## CPC

- H01M 4/366: {as layered products}
- C01B 32/21: After-treatment
- H01M 4/0471: {involving thermal treatment, e.g. firing, sintering, backing particulate active material, thermal decomposition, pyrolysis}
- H01M 4/133: Electrodes based on carbonaceous material, e.g. graphite-intercalation compounds or CFx
- H01M 4/587: for inserting or intercalating light metals
- H01M 4/60: of organic compounds
- H01M 4/622: {being polymers}
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- C01P 2002/74: by peak-intensities or a ratio thereof only
- C01P 2004/03: obtained by SEM
- C01P 2004/61: Micrometer sized, i.e. from 1-100 micrometer
- C01P 2006/10: Solid density
- C01P 2006/11: Powder tap density
- C01P 2006/12: Surface area
- C01P 2006/40: Electric properties
- H01M 4/1393: of electrodes based on carbonaceous material, e.g. graphite-intercalation compounds or CFx
- H01M 2004/027: {Negative electrodes}
- Y02E 60/10: Energy storage using batteries
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

The present application discloses a composite graphite material, a secondary battery, an apparatus and a preparation method thereof. The composite graphite material includes a core material and a coating layer coating at least a part of the surface of the core material, the core material including graphite; wherein the absolute value K of zeta potential of the composite graphite material in deionized water with a pH of 7 is at least 20 mV. The use of the composite graphite material provided by the present application can improve the cohesion and bonding force of the negative electrode plate, thereby reducing the cyclic expansion of the secondary battery.

## Claims

### Claim 1

A composite graphite material, comprising a core material and a coating layer coating at least a part of the surface of the core material, the core material comprising graphite,
wherein the composite graphite material has an absolute value K of Zeta potential of at least 20 mV, in deionized water with a pH of 7.

### Claim 2 (depends on 1)

The composite graphite material according to claim 1, wherein the absolute value K of zeta potential of the composite graphite material in deionized water with a pH of 7 is K≥25 mV, preferably 30 mV≤K≤40 mV.

### Claim 3 (depends on 1)

The composite graphite material according to claim 1, wherein the coating layer comprises a coating material containing a nitrogen-containing heterocyclic moiety, and at least a part of the nitrogen-containing heterocyclic moiety contains a carbon-nitrogen double bond, preferably the nitrogen-containing heterocyclic moiety further contains a carbon-carbon double bond.

### Claim 4 (depends on 3)

The composite graphite material according to claim 3, wherein the nitrogen-containing heterocyclic moiety comprises a fused aza-heterocyclic moiety;
preferably, the fused aza-heterocyclic moiety comprises one or more of Formula 1 to Formula 3:

### Claim 5 (depends on 3)

The composite graphite material according to claim 3, wherein when the temperature raises from 40° C. to 800° C., the composite graphite material has a weight loss rate in an inert non-oxidizing gas atmosphere of 0.1% to 0.55%, preferably from 0.1% to 0.4%, more preferably from 0.1% to 0.3%.

### Claim 6 (depends on 1)

The composite graphite material according to claim 1, wherein the core material is an artificial graphite.

### Claim 7 (depends on 6)

The composite graphite material according to claim 6, wherein the composite graphite material has a D peak intensity ID and a G peak intensity IG, and the ratio ID/IG is from 0.4 to 1.0, preferably from 0.6 to 0.85.

### Claim 8 (depends on 6)

The composite graphite material according to claim 6, wherein the composite graphite material satisfies: when the composite graphite material is in a electrode plate with a compaction density of 1.6 g/cm3 to 1.7 g/cm3, the ratio of the peak area C004 of 004 crystal plane to the peak area C110 of 110 crystal plane of the composite graphite material satisfies: C004/C110≤15, preferably 8≤C004/C110≤12.

### Claim 9 (depends on 6)

The composite graphite material according to claim 6, wherein the composite graphite material has a graphitization degree of 90% to 95%, preferably from 92% to 95%.

### Claim 10 (depends on 6)

The composite graphite material according to claim 6, wherein the composite graphite material also satisfies one or more of the following (1) to (7):
(1) the composite graphite material has a Dv50 of 15 μm to 20 μm, preferably from 15 μm to 18 μm;
(2) the composite graphite material has a Dv10 of at least 6 μm, preferably 6.5 μm≤Dv10≤10.5 μm;
(3) the composite graphite material has a Dn10 of 1.0 μm to 3.0 pin, preferably from 1.2 μm to 2.0 μm;
(4) the composite graphite material has a specific surface area SSA of 0.5 m2/g to 1.3 m2/g, preferably from 0.6 m2/g to 1.0 m2/g;
(5) the composite graphite material has a compacted powder density under a pressure of 5 tons of 1.80 g/cm3 to 2.10 g/cm3, preferably from 1.93 g/cm3 to 2.05 g/cm3;
(6) the composite graphite material has a tap density of 0.8 g/cm3 to 1.15 g/cm3, preferably from 0.9 g/cm3 to 1.05 g/cm3;
(7) the composite graphite material has a gram capacity of 350 mAh/g to 359 mAh/g, preferably from 352 mAh/g to 355 mAh/g.

### Claim 11 (depends on 1)

A secondary battery comprising a negative electrode plate which comprises a negative active material, wherein the negative active material comprises the composite graphite material according to claim 1.

### Claim 12 (depends on 11)

The secondary battery according to claim 11, wherein the negative electrode plate further comprises a binder including a copolymer, and the copolymer comprises at least a first monomer unit represented by Formula (I), a second monomer unit represented by Formula (II) and a third monomer unit represented by Formula (III),
wherein R1, R2, R3, R5, R6, R7, R9, R10, and R11 are each independently selected from hydrogen, a linear or branched alkyl group having 1 to 8 carbon atoms,
R4 is selected from hydrogen, a substituted or unsubstituted alkyl group having 1 to 8 carbon atoms,
R8 is selected from —COOM, sulfonate phenyl, and sodium sulfonate phenyl, and M is selected from H, and positive monovalent alkali metal ion,
R12 is selected from a substituted or unsubstituted alkyl group having 1 to 8 carbon atoms, and n is 0 or 1.

### Claim 13 (depends on 12)

The secondary battery according to claim 12, wherein, based on the total moles of the first monomer unit, the second monomer unit, and the third monomer unit, the first monomer unit is present in an amount of at least 40 mol %, preferably from 45 mol % to 85 mol %, more preferably from 60 mol % to 80 mol %; and/or,
based on the total moles of the first monomer unit, the second monomer unit and the third monomer unit, the second monomer unit is present in an amount of at most 29.5 mol %, preferably from 6 mol % to 28 mol %, more preferably from 8 mol % to 18 mol %; and/or,
based on the total moles of the first monomer unit, the second monomer unit and the third monomer unit, the third monomer unit is present in an amount of at most 30.5 mol %, preferably from 7.5 mol % to 30 mol %, more preferably from 12 mol % to 24 mol %.

### Claim 14 (depends on 11)

An apparatus comprising the secondary battery according to claim 11.

### Claim 15

A method for preparing a composite graphite material, comprising the step of coating at least a part of the surface of a core material comprising graphite with a coating material to obtain a composite graphite material;
wherein the composite graphite material has an absolute value K of zeta potential of at least 20 mV, in deionized water with a pH of 7.

### Claim 16 (depends on 15)

The method according to claim 15, wherein the step of coating at least a part of the surface of the core material with the coating material to obtain the composite graphite material comprises:
(1) mixing a solution containing a nitrogen-containing heterocyclizable polymer with a core material so that the polymer coats at least a part of the surface of the core material to obtain a slurry, wherein the core material comprises graphite, and a mass ratio of the core material to the polymer is mG:mP≤400:1;
(2) drying the slurry to obtain a staring material comprising a core material and a polymer layer coating at least a part of the surface of the core material;
(3) subjecting the starting material to heat treatment at a temperature of 300° C. to 400° C. for a heat treatment time of at least 2 hours, so that the polymer is heterocyclized to obtain a coating material with a fused aza-heterocyclic moiety, and at least part of the nitrogen-containing heterocycle in the fused aza-heterocyclic moiety has a carbon-nitrogen double bonds to obtain a composite graphite material.

### Claim 17 (depends on 16)

The method according to claim 16, wherein a mass ratio mG:mP of the core material to the polymer is from 30:1 to 400:1, preferably from 40:1 to 200:1, more preferably from 50:1 to 150:1.

### Claim 18 (depends on 16)

The method according to claim 16, wherein the polymer comprises one or more of polyacrylonitrile or copolymers thereof, and preferably polyacrylonitrile.

### Claim 19 (depends on 16)

The method according to claim 16, wherein the polymer has a number average molecular weight of 50,000 to 150,000, preferably from 80,000 to 120,000.

### Claim 20 (depends on 16)

The method according to claim 16, wherein, in the step (3),
the heat treatment of the starting material is performed at a temperature of 350° C. to 400° C.; and/or,
the heat treatment time is from 2 hours to 6 hours, preferably from 3 hours to 5 hours.