# US 2021/0280344 A1 · Method for preparing NdFeB magnet powder

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0280344 A1
- Document ID: US20210280344A1
- Status: Published application
- Kind: A1
- Application number: 17/131,810
- Filed: 2020-12-23
- Published: 2021-09-09
- Earliest claimed: 2019-12-31
- Assignees: Yantai Shougang Magnetic Materials Inc.
- Applicants: Yantai Shougang Magnetic Materials Inc
- Inventors: Xiulei CHEN; Zhongjie PENG; Xiaonan ZHU; Kaihong DING
- Web page: https://patentgrep.com/patent/US20210280344A1

## CPC

- B22F 9/023: {Hydrogen absorption}
- H01F 1/0571: {in the form of particles, e.g. rapid quenched powders or ribbon flakes}
- H01F 1/0573: {obtained by reduction or by hydrogen decrepitation or embrittlement}
- H01F 7/02: Permanent magnets {[PM]}
- B22F 1/052: characterised by a mixture of particles of different sizes or by the particle size distribution
- B22F 2009/044: {by jet milling}
- B22F 2203/00: Controlling
- B22F 2998/10: Processes characterised by the sequence of their steps
- C22C 38/00: Ferrous alloys, e.g. steel alloys (cast-iron alloys C22C37/00)
- C22C 2202/02: Magnetic
- B22F: WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER (making alloys by powder metallurgy C22C); APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

The present disclosure refers to a method of preparing a NdFeB magnet powder. The method includes a hydrogen treatment process including the steps of: a) charging NdFeB alloy flakes into a hydrogen treatment furnace, wherein the NdFeB alloy flakes include a neodymium-rich phase and a main phase; b) performing a hydrogen absorption by heating the hydrogen treatment furnace in a first stage to a temperature at which only the neodymium-rich phase undergoes a hydrogen absorption reaction, then introducing and maintaining hydrogen at a predetermined pressure until the hydrogen absorption of the neodymium-rich phase is finished, then stop heating of the hydrogen treatment furnace in a second stage, where the temperature falls to a temperature at which the main phase undergoes a hydrogen absorption reaction; and c) when the hydrogen absorption of step b) is finished, performing a vacuum dehydrogenation of the obtained coarse magnet powder.

## Claims

### Claim 1

A method of preparing a NdFeB magnet powder, the method including a hydrogen treatment process including the steps of:
a) charging NdFeB alloy flakes into a hydrogen treatment furnace, wherein the NdFeB alloy flakes include a neodymium-rich phase and a main phase;
b) performing a hydrogen absorption by heating the hydrogen treatment furnace in a first stage to a temperature at which only the neodymium-rich phase undergoes a hydrogen absorption reaction, then introducing and maintaining hydrogen at a predetermined pressure until the hydrogen absorption of the neodymium-rich phase is finished, then stop heating of the hydrogen treatment furnace in a second stage, where the temperature falls to a temperature at which the main phase undergoes a hydrogen absorption reaction; and
c) when the hydrogen absorption of step b) is finished, performing a vacuum dehydrogenation of the obtained coarse magnet powder.

### Claim 2 (depends on 1)

The method of claim 1, wherein, in the first stage of step b) of the hydrogen treatment process, the hydrogen treatment furnace is heated to a temperature between 390° C. to 480° C.

### Claim 3 (depends on 1)

The method of claim 1, wherein, in the first stage of step b) of the hydrogen treatment process, the heating to the temperature at which only the neodymium-rich phase undergoes the hydrogen absorption reaction is performed under argon and, when the temperature reaches said temperature, argon is removed from the hydrogen treatment furnace and hydrogen introduction is started.

### Claim 4 (depends on 2)

The method of claim 2, wherein, in the first stage of step b) of the hydrogen treatment process, the heating to the temperature at which only the neodymium-rich phase undergoes the hydrogen absorption reaction is performed under argon and, when the temperature reaches said temperature, argon is removed from the hydrogen treatment furnace and hydrogen introduction is started.

### Claim 5 (depends on 1)

The method of claim 1, wherein, in the first stage of step b) of the hydrogen treatment process, a hydrogen flow into the hydrogen treatment furnace is controlled such that a pressure in the hydrogen treatment furnace is maintained between 0.15 MPa to 0.20 MPa until the hydrogen flow stops.

### Claim 6 (depends on 2)

The method of claim 2, wherein, in the first stage of step b) of the hydrogen treatment process, a hydrogen flow into the hydrogen treatment furnace is controlled such that a pressure in the hydrogen treatment furnace is maintained between 0.15 MPa to 0.20 MPa until the hydrogen flow stops.

### Claim 7 (depends on 3)

The method of claim 3, wherein, in the first stage of step b) of the hydrogen treatment process, a hydrogen flow into the hydrogen treatment furnace is controlled such that a pressure in the hydrogen treatment furnace is maintained between 0.15 MPa to 0.20 MPa until the hydrogen flow stops.

### Claim 8 (depends on 4)

The method of claim 4, wherein, in the first stage of step b) of the hydrogen treatment process, a hydrogen flow into the hydrogen treatment furnace is controlled such that a pressure in the hydrogen treatment furnace is maintained between 0.15 MPa to 0.20 MPa until the hydrogen flow stops.

### Claim 9 (depends on 1)

The method of claim 1, wherein, in the second stage of step b) of the hydrogen treatment process, hydrogen is replaced by argon when the temperature is 220° C. or below, in particular when the temperature is below 130° C.

### Claim 10 (depends on 2)

The method of claim 2, wherein, in the second stage of step b) of the hydrogen treatment process, hydrogen is replaced by argon when the temperature is 220° C. or below, in particular when the temperature is below 130° C.

### Claim 11 (depends on 3)

The method of claim 3, wherein, in the second stage of step b) of the hydrogen treatment process, hydrogen is replaced by argon when the temperature is 220° C. or below, in particular when the temperature is below 130° C.

### Claim 12 (depends on 4)

The method of claim 4, wherein, in the second stage of step b) of the hydrogen treatment process, hydrogen is replaced by argon when the temperature is 220° C. or below, in particular when the temperature is below 130° C.

### Claim 13 (depends on 1)

The method of claim 1, wherein, in step c) of the hydrogen treatment process, the vacuum dehydrogenation is performed by heating to a temperature of 550° C. or more.

### Claim 14 (depends on 2)

The method of claim 2, wherein, in step c) of the hydrogen treatment process, the vacuum dehydrogenation is performed by heating to a temperature of 550° C. or more.

### Claim 15 (depends on 3)

The method of claim 3, wherein, in step c) of the hydrogen treatment process, the vacuum dehydrogenation is performed by heating to a temperature of 550° C. or more.

### Claim 16 (depends on 4)

The method of claim 4, wherein, in step c) of the hydrogen treatment process, the vacuum dehydrogenation is performed by heating to a temperature of 550° C. or more.

### Claim 17 (depends on 1)

The method of claim 1, wherein the NdFeB alloy flakes are prepared from raw materials by a strip casting process.

### Claim 18 (depends on 1)

The method claim 1, wherein a course magnetic powder obtained by the hydrogen treatment process is pulverized by a jet milling process.

### Claim 19 (depends on 18)

The method of claim 18, wherein a carrier gas of the jet milling process is nitrogen or argon.