# US 2021/0278142 A1 · Double-shell phase change heat storage balls and preparation method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0278142 A1
- Document ID: US20210278142A1
- Status: Published application
- Kind: A1
- Application number: 17/330,427
- Filed: 2021-05-26
- Published: 2021-09-09
- Earliest claimed: 2020-05-06
- Assignees: Wuhan University of Science and Technology
- Applicants: Wuhan University of Science and Technology
- Inventors: Huazhi Gu; Qiulin Xia; Meijie Zhang; Ao Huang; Lvping Fu; Fengming Zhou; Haifeng Li
- Web page: https://patentgrep.com/patent/US20210278142A1

## CPC

- F28D 20/023: {the latent heat storage material being enclosed in granular particles or dispersed in a porous, fibrous or cellular structure}
- C04B 35/117: Composites
- C04B 35/6263: {characterised by their solids loadings, i.e. the percentage of solids}
- C04B 35/6264: {Mixing media, e.g. organic solvents}
- C04B 35/62695: {Granulation or pelletising (devices for shaping artificial aggregates from ceramic mixtures B28B1/004)}
- C04B 35/6309: {Aluminium phosphates}
- C04B 35/636: Polysaccharides or derivatives thereof
- C04B 35/64: Burning or sintering processes (C04B33/32 takes precedence {; powder metallurgy B22F})
- C04B 35/66: Monolithic refractories or refractory mortars, including those whether or not containing clay {(making or repairing of linings F27D1/16)}
- C09K 5/063: {Materials absorbing or liberating heat during crystallisation; Heat storage materials}
- C04B 2235/3206: Magnesium oxides or oxide-forming salts thereof
- C04B 2235/3217: Aluminum oxide or oxide forming salts thereof, e.g. bauxite, alpha-alumina
- C04B 2235/3418: Silicon oxide, silicic acids or oxide forming salts thereof, e.g. silica sol, fused silica, silica fume, cristobalite, quartz or flint
- C04B 2235/3463: Alumino-silicates other than clay, e.g. mullite
- C04B 2235/349: Clays, e.g. bentonites, smectites such as montmorillonite, vermiculites or kaolines, e.g. illite, talc or sepiolite
- C04B 2235/48: Organic compounds becoming part of a ceramic after heat treatment, e.g. carbonising phenol resins
- C04B 2235/94: Products characterised by their shape
- C04B 2235/9607: Thermal properties, e.g. thermal expansion coefficient
- F28D 2020/0047: {using molten salts or liquid metals}
- Y02E 60/14: Thermal energy storage
- F28D: HEAT-EXCHANGE APPARATUS, NOT PROVIDED FOR IN ANOTHER SUBCLASS, IN WHICH THE HEAT-EXCHANGE MEDIA DO NOT COME INTO DIRECT CONTACT (fluid heaters having heat generating means and heat transferring means F24H; furnaces F27; details of heat-exchange apparatus of general)
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE
- C09K: MATERIALS FOR MISCELLANEOUS APPLICATIONS, NOT PROVIDED FOR ELSEWHERE
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

A double-shell phase change heat storage balls and preparation method thereof is disclosed. The technical scheme is as follows. Paraffin is placed in oven, and organic ignition loss is added to obtain paraffin melt containing the ignition loss; metal balls is immersed in the paraffin melt containing the ignition loss, and cooled naturally to obtain the metal balls coated by ignition loss and paraffin; alumina refractory slurry is placed in a pan granulator, and the metal balls coated by ignition loss and paraffin is added, pelletized, and dried to obtain alumina composite phase change heat storage ball bodies; mullite refractory slurry is placed in a pan granulator, alumina composite phase change heat storage ball bodies is added, pelletized, dried, and placed in a muffle furnace. The temperature is raised to 1200-1600° C. by three systems and maintained. After naturally cooling, the double-shell phase change heat storage balls are prepared.

## Claims

### Claim 1

A preparation method for a double-shell phase change heat storage balls, comprising:
Step 1: preparing raw materials with 50-70 wt % of a paraffin and 30-50 wt % of an organic ignition loss, placing the paraffin in an oven at 80-110° C. for 1-2 h to obtain a paraffin melt; then adding the organic ignition loss to produce a paraffin melt containing the ignition loss; then immersing metal balls in the paraffin melt containing the ignition loss for 10-20 s, and naturally cooling the immersed metal balls in a fume hood to prepare metal balls coated by ignition loss and paraffin;
Step 2: placing 15-35 wt % of an alumina refractory slurry in a pan granulator, then adding 65-85 wt % of the metal balls coated by ignition loss and paraffin into the pan granulator, rotating the pan granulator at 10-20 r/min for 0.5-1 h, taking out and placing the pelletized metal balls in a fume hood for 4-6 h, and then maintaining a temperature at 80-110° C. for 20-24 h to prepare alumina composite phase change heat storage ball bodies;
Step 3: placing 25-40 wt % of a mullite refractory slurry in a pan granulator, then adding 60-75 wt % of the alumina composite phase change heat storage ball bodies into the pan granulator, rotating the pan granulator at 10-20 r/min for 0.5-1 h, taking out and placing the pelletized ball bodies in a fume hood for 4-6 h, and then placing in an oven, maintaining at 80-110° C. for 20-24 h to prepare an alumina-mullite double-shell phase change heat storage ball bodies;
Step 4: placing the alumina-mullite double-shell phase change heat storage ball bodies in a muffle furnace, increasing a temperature to 500-550° C. at a rate of 5-10° C./min, maintaining the temperature for 2-4 h, then increasing the temperature to 850-1100° C. at a rate of 3-5° C./min, maintaining the temperature for 3-5 h, then increasing the temperature to 1200-1600° C. at a rate of 2-5° C./min, maintaining the temperature for 3-5 h, and naturally cooling to room temperature to produce double-shell phase change heat storage balls;
wherein a preparation method for the alumina refractory slurry comprises:
premixing 80-90 wt % of a corundum fine powder, 3-5 wt % of an α-alumina powder, 4-8 wt % of a Guangxi clay, 1-3 wt % of a silica fine powder, 1-2 wt % of a calcium lignosulphonate and 1-2 wt % of a dextrin to obtain a premix; then adding 6-8 wt % of an aluminum dihydrogen phosphate solution and 8-10 wt % of water to the premix and stirring uniformly to prepare the alumina refractory slurry; and
a preparation method for the mullite refractory slurry comprises:
premixing 68-82 wt % of a mullite fine powder, 6-10 wt % of an α-alumina powder, 4-8 wt % of a Guangxi clay, 5-9 wt % of a silica fine powder, 1-2 wt % of a calcium lignosulphonate and 2-3 wt % of a dextrin to obtain a premix; then adding 6-8 wt % of an aluminum dihydrogen phosphate solution and 8-10 wt % of water to the premix and stirring uniformly to prepare the mullite refractory slurry.

### Claim 2 (depends on 1)

The preparation method for the double-shell phase change heat storage balls of claim 1, wherein the organic ignition loss is one kind of starch, sawdust and rice bran husk, and a particle size of the organic ignition loss is less than or equal to 180 μm.

### Claim 3 (depends on 1)

The preparation method for the double-shell phase change heat storage balls of claim 1, herein the metal balls are one kind of aluminum balls, aluminum silicon alloy balls, aluminum silicon iron alloy balls, aluminum silicon nickel alloy balls and silicon magnesium alloy balls, and a particle size of the metal balls is 5-30 mm;
an Al content of the aluminum balls is greater than or equal to 97 wt %;
an Al content of the aluminum silicon alloy balls is greater than or equal to 56 wt %, and an Si content of the aluminum silicon alloy balls is greater than or equal to 40 wt %;
an Al content of the aluminum silicon iron alloy balls is 45˜60 wt %, an Si content of the aluminum silicon iron alloy balls is 30˜40 wt %, and an Fe content of the aluminum silicon iron alloy balls is 5˜15 wt %;
an Al content of the aluminum silicon nickel alloy balls is 30˜40 wt %, an Si content of the aluminum silicon nickel alloy balls is 40˜50 wt %, and an Ni content of the aluminum silicon nickel alloy balls is 20˜30 wt %; and
an Mg content of the silicon magnesium alloy balls is 40˜80 wt %, and an Si content of the silicon magnesium alloy balls is 50˜60 wt %.

### Claim 4 (depends on 1)

The preparation method for the double-shell phase change heat storage balls of claim 1, wherein an Al2O3 content of the corundum fine powder is greater than or equal to 98 wt %; and a particle size of the corundum fine powder is less than or equal to 74 μm.

### Claim 5 (depends on 1)

The preparation method for the double-shell phase change heat storage balls of claim 1, wherein an Al2O3 content of the α-alumina powder is greater than or equal to 97 wt %; and a particle size of the α-alumina powder is less than or equal to 8 μm.

### Claim 6 (depends on 1)

The preparation method for the double-shell phase change heat storage balls of claim 1, wherein an Al2O3 content of the Guangxi clay is 33-36 wt %, a SiO2 content of the Guangxi clay is 46-49 wt %, and a Fe2O3 content of the Guangxi clay is 1-1.3 wt %;
and a particle size of the Guangxi clay is less than or equal to 180 μm.

### Claim 7 (depends on 1)

The preparation method for the double-shell phase change heat storage balls of claim 1, wherein a SiO2 content of the silica fine powder is greater than or equal to 92 wt %; and a particle size of the silicon fine powder is less than or equal to 0.6 μm.

### Claim 8 (depends on 1)

The preparation method for the double-shell phase change heat storage balls of claim 1, wherein a P2O5 content of the aluminum dihydrogen phosphate solution is greater than or equal to 33 wt %; and an Al2O3 content of the aluminum dihydrogen phosphate solution is greater than or equal to 8 wt %.

### Claim 9 (depends on 1)

The preparation method for the double-shell phase change heat storage balls of claim 1, wherein an Al2O3 content of the mullite fine powder is greater than or equal to 68 wt %; and a particle size of the mullite fine powder is greater than or equal to 0.088 mm.

### Claim 10 (depends on 1)

A double-shell phase change heat storage balls, wherein the double-shell phase change heat storage balls are double-shell phase change heat storage balls prepared by the preparation method for double-shell phase change heat storage balls of claim 1.