# US 2021/0277513 A1 · Method of Preparing ITO Ceramic Target With Controllable Grain Size

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0277513 A1
- Document ID: US20210277513A1
- Status: Published application
- Kind: A1
- Application number: 15/930,912
- Filed: 2020-05-13
- Published: 2021-09-09
- Earliest claimed: 2020-03-06
- Assignees: Zhengzhou University
- Applicants: Zhengzhou University
- Inventors: Jilin HE; Benshuang SUN; Yongchun SHU; Yang LIU; Jie CHEN; Xueyun ZENG
- Web page: https://patentgrep.com/patent/US20210277513A1

## CPC

- C04B 35/6263: {characterised by their solids loadings, i.e. the percentage of solids}
- C23C 14/3414: {Metallurgical or chemical aspects of target preparation, e.g. casting, powder metallurgy}
- C04B 35/457: based on tin oxides or stannates
- C04B 35/6261: {Milling}
- C04B 35/634: Polymers (C04B35/636 takes precedence)
- C04B 35/63416: {Polyvinylalcohols [PVA]; Polyvinylacetates}
- C04B 35/63424: {Polyacrylates; Polymethacrylates}
- C04B 35/63444: {Nitrogen-containing polymers, e.g. polyacrylamides, polyacrylonitriles, polyvinylpyrrolidone [PVP], polyethylenimine [PEI]}
- C04B 35/63468: {Polyamides}
- C04B 35/636: Polysaccharides or derivatives thereof
- C04B 35/638: Removal thereof
- C04B 35/64: Burning or sintering processes (C04B33/32 takes precedence {; powder metallurgy B22F})
- C04B 2111/00224: {Green materials, e.g. porous green ceramic preforms}
- C04B 2235/3286: Gallium oxides, gallates, indium oxides, indates, thallium oxides, thallates or oxide forming salts thereof, e.g. zinc gallate
- C04B 2235/3293: Tin oxides, stannates or oxide forming salts thereof, e.g. indium tin oxide [ITO]
- C04B 2235/5445: submicron sized, i.e. from 0,1 to 1 micron
- C04B 2235/5454: nanometer sized, i.e. below 100 nm
- C04B 2235/604: Pressing at temperatures other than sintering temperatures
- C04B 2235/608: Green bodies or pre-forms with well-defined density
- C04B 2235/6562: Heating rate
- C04B 2235/6565: Cooling rate
- C04B 2235/6567: Treatment time
- C04B 2235/77: Density
- C04B 2235/786: Micrometer sized grains, i.e. from 1 to 100 micron
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)

## Abstract

A method of preparing an ITO ceramic target includes that: In2O3 powder with mass fraction of 90˜97 and SnO2 powder with mass fraction of 10˜3 are ball-milled and mixed with deionized water, diluent, binder and polymer material by a sand mill to obtain an ITO ceramic slurry with a solid content between 70˜80% and a viscosity between 120˜300 mpa·s, with an average particle size D50 of the mixed powder controlled at 100˜300 nm; the ITO ceramic slurry is shaped by a pressure grouting to obtain an ITO ceramic green body with a relative density of 58˜62%; the ITO ceramic green body is put into a degreasing and sintering integrated furnace, and under a degreasing temperature of 700˜800° C., the ITO ceramic target is degreased in an atmospheric oxygen atmosphere for the time set to 12˜36 hours; the temperature increases from the degreasing temperature to the first sintering temperature of 1,600˜1,650° C.

## Claims

### Claim 1

A method of preparing an ITO ceramic target with a controllable grain size, comprising:
ball-milling and mixing In2O3 powder with mass fraction of 90˜97 and SnO2 powder with mass fraction of 10˜3, with deionized water, diluent, binder and polymer material, by a sand mill to obtain an ITO ceramic slurry with a solid content between 70˜80% and a viscosity between 120˜300 mpa·s, with an average particle size D50 of the mixed powder in the ITO ceramic slurry controlled at 200·300 nm;
shaping the ITO ceramic slurry by a pressure grouting to obtain an ITO ceramic green body with a relative density of 58˜62%;
the ITO ceramic green body undergoing an integrated degreasing and sintering treatment to obtain the ITO ceramic target; wherein, the integrated degreasing and sintering treatment includes:
putting the ITO ceramic green body into a degreasing and sintering integrated furnace;
heating the degreasing and sintering integrated furnace to a degreasing temperature of 700˜800° C., degreasing the ITO ceramic target in an atmospheric oxygen atmosphere for a degreasing time set to 12 to 36 hours;
increasing the degreasing and sintering integrated furnace from the degreasing temperature to a first sintering temperature of 1,600˜1,650° C.; and
after increasing to the first sintering temperature, keeping temperature at the first sintering temperature for 0˜60 min, then starting to reduce the degreasing and sintering integrated furnace from the first sintering temperature to a second sintering temperature of 1,500˜1,540° C., and sintering the ITO target at the second sintering temperature in the atmospheric oxygen atmosphere, with temperature kept for 12 to 36 hours, to finally obtain the ITO ceramic target.

### Claim 2 (depends on 1)

The method according to claim 1, wherein the mass fractions of In2O3 powder and SnO2 powder are 90 and 10.

### Claim 3 (depends on 1)

The method according to claim 1, wherein the mass fractions of In2O3 powder and SnO2 powder are 95 and 5.

### Claim 4 (depends on 1)

The method according to claim 1, wherein the mass fractions of In2O3 powder and SnO2 powder are 93 and 7.

### Claim 5 (depends on 1)

The method according to claim 1, wherein a primary particle size distribution range of the In2O3 powder is 80˜200 nm, and a primary particle size distribution range of the SnO2 powder is 80˜200 nm.

### Claim 6 (depends on 1)

The method according to claim 1, wherein the diluent includes polyacrylic or polycarboxylic acid diluent, the binder includes gum arabic, polyvinyl alcohol or acrylic resin, and the polymer material includes polyacrylamide.

### Claim 7 (depends on 1)

The method according to claim 1, wherein said ball-milling and mixing is performed under vacuum depressurized conditions, the negative pressure not greater than 9 Pa.

### Claim 8 (depends on 1)

The method according to claim 1, wherein a heating rate from a room temperature to the degreasing temperature is set to 1˜3° C./min.

### Claim 9 (depends on 1)

The method according to claim 1, wherein a heating rate from the degreasing temperature to the first sintering temperature is set to 2˜5° C./min.

### Claim 10 (depends on 1)

The method according to claim 1, wherein a cooling rate from the first sintering temperature to the second sintering temperature is set to 8˜16° C./min.