# US 2021/0262069 A1 · Flat Steel and Method for Producing Same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2021/0262069 A1
- Document ID: US20210262069A1
- Status: Published application
- Kind: A1
- Application number: 17/251,302
- Filed: 2019-06-12
- Published: 2021-08-26
- Earliest claimed: 2018-06-12
- Assignees: ThyssenKrupp Steel Europe AG; thyssenkrupp AG
- Applicants: ThyssenKrupp Steel Europe AG; thyssenkrupp AG
- Inventors: Manuela Irnich; Rainer Fechte-Heinen; Miriam Lange; Bernd Linke; Jan-Hendrik Rudolph; Richard G. Thiessen
- Web page: https://patentgrep.com/patent/US20210262069A1

## CPC

- C21D 9/48: deep-drawing sheets
- C22C 38/04: containing manganese
- C21D 8/04: to produce plates or strips for drawing, e.g. for deep-drawing
- C21D 8/0426: {Hot rolling}
- C21D 8/0436: {Cold rolling}
- C21D 8/0447: {characterised by the heat treatment}
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/06: containing aluminium
- C22C 38/20: with copper
- C22C 38/22: with molybdenum or tungsten
- C22C 38/24: with vanadium
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/32: with boron
- C22C 38/38: with more than 1.5% by weight of manganese
- C22C 38/40: with nickel
- C23G 1/00: Cleaning or pickling metallic material with solutions or molten salts (with organic solvents C23G5/02)
- C21D 2211/001: Austenite
- C21D 2211/002: Bainite
- C21D 2211/004: Dispersions; Precipitations
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- C23C 2/06: Zinc or cadmium or alloys based thereon
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23G: CLEANING OR DE-GREASING OF METALLIC MATERIAL BY CHEMICAL METHODS OTHER THAN ELECTROLYSIS
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)

## Abstract

A flat steel product consisting of (in wt %) 0.1-0.5% C, 1.0-3.0% Mn, 0.9-1.5% Si, ≤1.5% Al, ≤0.008% N, ≤0.020% P, ≤0.005% S, 0.01-1% Cr and optionally one or more of: ≤0.2% Mo, ≤0.01% B, ≤0.5% Cu, ≤0.5% Ni and optionally a total of 0.005-0.2% microalloying elements, the remainder iron and unavoidable impurities. The steel has a structure consisting of ≥80 area % martensite, where ≥75 area % is tempered and ≤25 area % is non-tempered, ≥5 volume % residual austenite, 0.5-10 area % ferrite, ≤5 area % bainite, and carbides with a length of ≤250 nm, wherein in the phase boundary between tempered martensite and residual austenite, there is a low-Mn ferrite seam having a width of 4·12 nm and a Mn content of ≤50% of the average Mn content. Also, a method for producing the flat steel in which the structural characteristics of the flat steel product are set by suitable heat treatment.

## Claims

### Claim 1

A flat steel product consisting of (in wt %)
0.1-0.5%
C,
1.0-3.0%
Mn,
0.9-1.5%
Si,
up to 1.5%
Al,
up to 0.008%,
N,
up to 0.020%,
P,
up to 0.005%,
S,
0.01-1%
Cr,
as well as optionally consisting of one or more of the following elements
up to 0.2%
Mo,
up to 0.01%
B,
up to 0.5%
Cu,
up to 0.5%
Ni
as well as optionally consisting of in total 0.005-0.2% microalloying elements and iron as a remainder and unavoidable impurities, wherein the following applies:
75≤(Mn2+55*Cr)/Cr≤3000
where Mn is the Mn content of the steel in wt %, and Cr is the Cr content of the steel in wt %,
the flat steel product having a structure, consisting of
at least 80 area % martensite, of which
at least 75 area % is tempered martensite and at most 25 area % is non-tempered martensite,
at least 5% by volume residual austenite,
0.5 to 10 area % ferrite and
at most 5 area % bainite,
wherein in a region of a phase boundary between tempered martensite and residual martensite, there is a low-Mn ferrite seam which has a width of at least 4 nm and at most 12 nm and a Mn content of at most 50% of the average total Mn content of the flat steel product and
wherein the flat steel product has carbides, and a length of the carbides are equal to or less than 250 nm.

### Claim 2 (depends on 1)

The flat steel product according to claim 1, wherein the flat steel product has a tensile strength of 900 to 1500 MPa, a yield strength Rp02 of more than 700 MPa, an elongation A80 of 7 to 25%, a bending angle of greater than 80°, a hole expansion of greater than 25% and a maximum deep-drawing ratio βmax for which the following applies:
βmax≥−1.9·10−6×(Rm)2+3.5·10−3×Rm+0.5
where Rm is the tensile strength of the flat steel product in MPa.

### Claim 3 (depends on 1)

A flat steel product according to claim 1, wherein the width of the low-Mn ferrite seam is at least 8 nm.

### Claim 4 (depends on 1)

The flat steel product according to claim 1, wherein the width of the low-Mn ferrite seam is at most 10 nm.

### Claim 5 (depends on 1)

The flat steel product according to claim 1, wherein the Mn content of the low-Mn ferrite seam is at most 30% of the average total Mn content of the flat steel product.

### Claim 6 (depends on 1)

The flat steel product according claim 1, wherein the length of the carbides is less than 175 nm.

### Claim 7 (depends on 2)

The flat steel product according to claim 2, wherein the flat steel product has a maximum deep-drawing ratio β of at least 1.475.

### Claim 8 (depends on 1)

The flat steel product according claim 1, wherein the flat steel product is provided with a metallic coating.

### Claim 9

A method for producing a high-strength flat steel product, comprising at least the following work steps:
a) Providing a slab consisting of, in addition to iron and unavoidable impurities, (in wt %)
0.1-0.5% C, 1.0-3.0% Mn, 0.9-1.5% Si, up to 1.5% Al, up to 0.008% N, up to 0.020% P, up to 0.005% S, 0.01 to 1% Cr, as well as optionally consisting of one or more of the following elements: up to 0.2% Mo, up to 0.01% B, up to 0.5% Cu, up to 0.5% Ni as well as optionally consisting of in total 0.005-0.2% of microalloying elements, wherein the following applies: 75≤(Mn2+55*Cr)/Cr≤3000 where Mn is the Mn content of the steel in wt %, Cr is the Cr content of the steel in wt %;
b) Heating the slab to a temperature of 1000-1300° C. and hot rolling the slab into a hot strip, wherein the end rolling temperature T_ET is greater than 850° C.;
c) Cooling the hot strip within at most 25 seconds to a coiling temperature T_HT of 400 to 620° C., and winding the hot strip into a coil;
d) Pickling the hot-rolled flat steel product;
e) Cold-rolling the hot-rolled flat steel product;
f) Heating the cold-rolled flat steel product to a holding zone temperature T_HZ of at least 15° C. above the A3 temperature of the flat steel product and is at most 950° C., wherein the heating takes place either
f1) in one phase at an average heating rate of 2-10 K/s
or
f2) in two phases at a first heating speed Theta_H1 of 5-50 K/s up to a conversion temperature T_W of 200-400° C. and above the conversion temperature T_W at a second heating speed Theta_H2 of 2-10 K/s;
g) Holding the flat steel product for a duration t_HZ of 5-15 seconds at the holding zone temperature T_HZ;
h) Cooling the flat steel product from the holding zone temperature T_HZ to a cooling stop temperature T_Q that is between the martensite start temperature T_MS and a temperature that is 175° C. lower than T_MS, at either
h1) a cooling rate Theta_Q1 which is at least 30 K/s;
or
h2) a first cooling rate Theta_LK of less than 30 K/s for a first cooling to an intermediate temperature T_LK of not lower than 650° C., and a second cooling rate Theta_Q2 for a second cooling from T_L to T_Q, wherein Theta_Q2 is at least 30 K/s;
i) Holding the flat steel product at the cooling stop temperature T_Q for 1-60 seconds;
j) Heating the flat steel product at a first heating rate Theta_B1 of between 5 and 100 K/s, to a first treatment temperature T_B1 of at least T_Q+10° C. and at most 450° C., holding the flat steel product at the first treatment temperature T_B1 for a duration t_B1 of 8.5 seconds to 245 seconds, heating the flat steel product at a second heating rate Theta_B2 of between 2 and 50 K/s, to a second treatment temperature T_B2 of at least T_B1+10° C. and at most 500° C., optionally isothermically holding the flat steel product at the treatment temperature T_B2 for a duration t_B2 of up to 34 seconds, wherein the entire treatment time t_B2 for the heating and the isothermic holding is in total between 10 and 250 seconds;
k) Optionally coating the flat steel product in a Zn-based coating bath;
l) Cooling the flat steel product to room temperature at a cooling rate Theta_B3 of at least 5 K/s.

### Claim 10 (depends on 9)

The method according to claim 9, a weight of the hot strip wound into a coil is at least 10 tons.

### Claim 11 (depends on 9)

The method according to claim 9, wherein the hot strip is cooled in work step c) within at most 18 seconds.

### Claim 12 (depends on 9)

The method according to claim 9, wherein the coiling temperature T_HT is at most 600° C.

### Claim 13 (depends on 9)

The method according to claim 9, wherein the hold time t_Q is at least 5 seconds.

### Claim 14 (depends on 9)

The method according to claim 9, wherein the cooling stop temperature T_Q is between a temperature that is lower than the martensite start temperature T_MS by 75° C., and a temperature that is lower than T_MS by 150° C.

### Claim 15 (depends on 9)

The method according to claim 9, wherein the duration t_BR2 for the heating to T_B2 and the duration for the optional holding at T_B2 is together at most 35 seconds.